Audio player docked to bottom

Listen to this article
Hydrogen, methane or ethane up, no acetylene? Stray gassing may explain the DGA, but it is not an all-clear. On this unit it has to be shown that its oil can make this gas, with partial discharge and thermal faults investigated, and even then whether anything in the unit ran hotter than usual remains open.
At a glance
- What it is. IEC 60296:2020 defines stray gassing as gas the liquid makes at usual service temperatures, not the product of an internal fault; CIGRE TB 771:2019 reads the same gas as an indication of abnormal oil temperature somewhere inside the transformer.
- What it means: a symptom, not noise, and not an all-clear. The first half is CIGRE TB 771's reading (App. G.2, p. 61). The second is ours: stray gassing has to be shown on this unit's oil, with partial discharge and thermal faults investigated; offered instead of an investigation, it is only a hypothesis.
- What to look at. There is no single fingerprint: depending on the oil, hydrogen or ethane leads. Ratios and Duval zones are an indication, never the decision.
- What to test. If stray gassing is put forward as the explanation, it needs a stray-gassing test on oil from this transformer. The test characterises the oil, not the transformer.
- How urgent. That depends on this unit's gas levels, trend and history, not on the name. What the standards recommend as gas levels rise is in What the standards recommend; CIGRE's hydrogen levels for stray gassing are in What the standards recommend: the ladder and TB 771's levels.
TriboTech is an independent consultancy in transformer-oil analysis and DGA. General information: a judgement on a unit needs its data and history; where the conclusion is ours, we say so.
What stray gassing is, and where the sources differ
IEC 60296:2020 defines stray gassing as the formation of gases, such as hydrogen, methane or ethane, from an insulating liquid's own constituents, in service. By IEC 60296's definition it forms at temperatures considered usual for normal operation and is not connected to an internal fault in the equipment (Cl. 6.19, p. 20). CIGRE notes that, depending on the oil, stray gassing may be mistaken for corona partial discharge (PD) or for a T1 or T2 thermal fault (TB 296:2006, § 3.5, p. 15). IEC 60599 places T1 below 300 °C and T2 from 300 to 700 °C (IEC 60599:2022, Table 1, p. 14).
A non-damage fault: a classification, not a dismissal. IEC 60599 classes stray gassing as a non-damage fault. In that standard a fault is an "unplanned occurrence or defect in an item which may result in one or more failures". A non-damage fault is a "fault which does not involve repair or replacement action at the point of the fault". IEC 60296 uses the word the other way round, in the definition above (IEC 60599, Cl. 4.3, p. 12; Cl. 3.1.1, p. 8; Cl. 3.1.2, p. 9; IEC 60296, Cl. 6.19, p. 20; the two uses of "fault").
Whether anything in the unit ran hotter than usual is still to be shown. If the gas is shown to be stray gassing, IEC 60599 classes it as a non-damage fault, one with no repair or replacement at the point where it forms.
CIGRE's 2024 brochure puts the state of knowledge plainly: after more than ten years the phenomenon "seems to be quite far from being fully elucidated". It "has no clearly defined borders, and strongly depends on the procedure used to evaluate it". TB 927 concludes that CIGRE's first, thermal definition should be extended (CIGRE TB 927:2024, § 1.3, p. 12; § 1.5, p. 13; how the definition changed).
Reference How the definition changed, and the borders of the term
CIGRE TB 296:2006 defined stray gassing first, as gas formed in insulating mineral oils heated at relatively low temperatures, 90–200 °C (§ 3, p. 11). TB 771:2019 describes itself as a continuation of that work and keeps the definition (Executive summary, p. 5; App. G.1, p. 61), and IEC 60599:2022 still cites TB 296 for the definition and the evaluation method (Cl. 4.3, p. 12, ref. [3]). IEC 60599 cites it with the upper bound only and adds oil oxidation (Cl. 4.3, p. 12), and settles the status: "Stray gassing is a non-damage fault" (Cl. 4.3, p. 12). TB 927 says the first definition gives stray gassing "a purely "thermal" meaning" (§ 1.3, p. 12). IEC 60296:2020 dropped the temperature range and tied it to the equipment instead (Cl. 6.19, p. 20). Because air also accelerates the gas formation, TB 927 assumes stray gassing to be "a thermo-oxidative process rather than a merely thermal one", and concludes that "the definition given by TF11 should be extended" (§ 1.3, p. 12; § 1.5, p. 13). IEC 60296:2020 defines "stray gassing under thermo-oxidative stress" at "temperatures considered usual for normal operating conditions" (Cl. 6.19, p. 20).
One view of why oil makes gas: for mineral oil, the field paper's authors put it down to the chemical instability of oil molecules after refining. Hydrogen treatment, for example, may oversaturate the hydrocarbon chains with hydrogen, which is released as H₂, with some C₂H₆ and CH₄, when the oil is heated or in contact with oxygen (Buchacz et al. 2021, § 1, p. 1729).
Arguing against a mandatory limit for new oil, TB 771 wrote that such a limit "may unduly reject some oils which otherwise would be totally acceptable in terms of functional properties (electrical insulation, cooling, etc)", and that "it may result in litigations between transformer users and manufacturers, since stray gas formation in service above 105°C may be attributed wrongly to a transformer design problem rather than to the oil"; limits "should therefore be left to oil users, not to standardization bodies to decide" (App. G.7, p. 66). In the same appendix TB 771 reads stray gases as "an indication of abnormal oil temperature somewhere inside the transformer (not supposed to exceed ~105°C in transformer loading guides), due to design or operational problems, which may or may not need to be fixed after discussions with the transformer manufacturer" (App. G.2, p. 61). The brochure does not reconcile the two. Read together (our reading): the gas alone does not say what is behind it; that has to be shown on the unit. IEC published a limit for Type A oil (IEC 60296:2020, Table 3, p. 21).
The two IEC standards do not use "fault" alike. In IEC 60599 a fault is an "unplanned occurrence or defect in an item which may result in one or more failures of the item itself or of other associated equipment" (Cl. 3.1.1, p. 8). In our view the qualifier "non-damage" removes the repair, nothing else. Read together, in our view, whether anything in the unit ran hotter than usual is a question neither standard answers for a given unit.
What IEC 60296 and CIGRE keep outside the term:
- Gassing tendency, a separate property in IEC 60296 (Cl. 7.3, p. 24): whether the oil evolves or absorbs gas under an electric discharge through a gas phase at a gas–oil interface (IEC 60628:1985, Cl. 1, p. 7).
- Gas from incompatible materials, such as paints or some types of cross-linked polyethylene, which IEC 60296 excludes from its definition by name (Cl. 6.19, p. 20), and gas "provoked or catalyzed by external factors", which CIGRE says "should not be considered in the definition of stray gassing" (TB 927, § 1.5, p. 13).
- Catalytic reactions on metal surfaces or paints, which TB 296 warns not to confuse with it (§ 3, p. 11).
Other documents draw the border wider. IEC 63585 speaks of "stray gassing caused by the insulating liquid itself or the used construction materials or some additives (like metal passivators)" (Cl. 5.3.6, p. 19). ASTM D7150 defines it as "the production of gases in an insulating liquid due to heating, contamination or in combination" (Cl. 3.1.1, p. 1). CIGRE notes that in practice the term "is used rather broadly to refer to gases present in equipment (when doing DGA) that are not believed to be due to an electrical or thermal fault" (TB 927, § 1.2.2, p. 11).
In our view, whatever it is called, gas from materials in the unit is not a property of the oil.
Where the sources stand, question by question:
- What counts as stray gassing? Sources differ. IEC 60296 keeps incompatible materials out of its definition, and CIGRE TB 927 keeps out gas provoked or catalysed by external factors. IEEE C57.104 says it could also occur due to incompatibility between materials, IEC 63585 names the construction materials used, and ASTM D7150 includes contamination (IEC 60296, Cl. 6.19, p. 20; TB 927, § 1.5, p. 13; IEEE C57.104, Annex C.2, p. 59; IEC 63585, Cl. 5.3.6, p. 19; ASTM D7150, Cl. 3.1.1, p. 1).
- At what temperature does it form? Sources differ. From ranges that end at 200 °C (TB 296, TB 771, IEC 60599, IEEE C57.104) to temperatures considered usual for normal operation (IEC 60296). In the laboratory, a certain gas formation may appear down to 40–45 °C if the test runs long enough (TB 927). IEEE C57.104 prints below 200 °C (Annex C.2, p. 59); Figure 3 gives the other sources in their own words, with their pages.
- Does the gas mean something in the unit ran hot? Sources differ. TB 771 reads stray gases as an indication of abnormal oil temperature somewhere inside the transformer. TB 927: stray gassing "can take place at normal operating transformer temperatures" (TB 771, App. G.2, p. 61; TB 927, § 2, p. 24).
- Is it a fault? Sources differ. IEC 60296 defines it as not connected to an internal fault in the electrical equipment. IEC 60599: "Stray gassing is a non-damage fault". IEEE C57.104 lists it, in an informative annex, as fault sub-type S (IEC 60296, Cl. 6.19, p. 20; IEC 60599, Cl. 4.3, p. 12; IEEE C57.104, Annex C.2, p. 59); its main text is quoted under Is stray gassing harmful?.
- Why does the oil do it? Not known. TB 296: "The mechanisms of stray gas formation are not known for sure". IEC 60296 gives refining and additives as examples of possible causes, and oxygen, copper and temperature as accelerators (TB 296, § 3.2, p. 13; IEC 60296, Cl. 6.19, p. 20).
- Is it harmful? Not known. Among the cases reported to CIGRE's working group, no failure due to stray gassing was reported. IEC 60296: "In practice, gas due to stray gassing only has not been proven to be harmful to the equipment". For a unit in DGA Status 2 (IEEE's middle status of three, set by gas levels, deltas and rates) whose fault diagnosis reveals PD, T1 or stray gassing, IEEE C57.104: "a less urgent issue, but still may affect future life of the insulation system" (TB 771, § 3.2, p. 17; IEC 60296, Cl. 6.19, p. 20; IEEE C57.104, Cl. 6.1.2.2, p. 36). Is stray gassing harmful? gives them in context.
- Does a laboratory test predict the unit? Sources differ. TB 296: "In most cases, there is no correlation" between test results at 120 °C and field gassing in the first year(s) of service. TB 927 observed similar gassing patterns of the same oil types in tests and transformer DGA, yet writes that there is "no criteria to compare this gassing to the eventual stray gassing of the oil" (TB 296, § 3.3, p. 13; TB 927, § 1.1, p. 9; § 1.4, p. 13).
Our view: a term without clear borders settles nothing by being named. Whether this unit's gas is stray gassing, and whether anything in the unit ran hotter than usual, both have to be shown on this unit's oil and against its history.
One case: the washers in unit 2-T2
In 2016 a 115 kV, 63 MVA transformer carried 11 150 ppm of hydrogen, in or near the partial-discharge zone of Duval Pentagon 2 (Duval's mineral-oil pentagon; splits the thermal zones into S, O, C, T3-H). Partial-discharge testing found only a very weak signal (Buchacz, Buchacz & Duval 2021, pp. 1730–1731). It was inspected in 2017 because of its hydrogen; galvanised steel washers were found at an electrical connection and removed, and by 2020 its hydrogen was 5 ppm (p. 1731). The authors write that the hydrogen cannot be attributed to corona PDs in the washers, and judge overheating of the washers, with stray gassing of the oil in contact with them, much more likely (p. 1734). After these findings and laboratory tests on the units' oil (pp. 1730–1733), the authors attribute the gas in the two families they studied to stray gassing of oil "between 90 °C and 180 °C depending on the individual units". The authors conclude: "Such SG of oil is not a concern for the safe operation of these transformers" (p. 1734). Our view: on either definition, the authors placed the source of the gas in the unit, and an inspection found the washers.
The oil change, the degassing and the definitions the authors use are in the case in detail.
Reference The washer case in detail
2-T2's oil had been changed two years before 2016, and its gas pattern was the same as in its five sister units on the original oil (Buchacz, Buchacz & Duval 2021, pp. 1730–1731). After the sister units' oil had been degassed in 2016, "their gassing patterns occur at the same place" (p. 1731). The authors use CIGRE's definition of stray gassing, gas from oil heated at relatively low temperatures of 90 to 200 °C, not IEC 60296's narrower one (p. 1729; IEC 60296, Cl. 6.19, p. 20).
The paper reports two families, and they end differently. In the first the ethane reached 112 ppm and the laboratory patterns matched at about 160 °C, which the authors attribute to hot metal in the oil. CIGRE gives 550 ppm of ethane as the typical concentration level for overheating faults below 250 °C (TB 771, Table 3.4, p. 19); the authors call 112 ppm very much below that, and conclude that those units can be left in service using normal sampling intervals (e.g., every year) (Buchacz, p. 1734). The washer family is the second. For 2016 the text on p. 1731 and the paper's Fig. 6 table both give 11 150 ppm; the text gives 11 500 ppm as the level behind the 2017 inspection.
The authors write that the hydrogen "cannot be attributed to corona PDs in the washers", and that it is "much more likely due to overheating of the washers because of their poor electrical conductivity, subsequent overheating, and SG of the oil in contact with them" (p. 1734). In 2020 an acoustic PD test on one of the sister units, 2-T5, found "very weak PDs deep inside its active part in phase W, not in the washers" (p. 1731). Their abstract states the conclusion more broadly, "according to observations published by CIGRE" (p. 1729).
The authors read about 90 °C for the washers from the gas patterns. The pattern in service lay between their laboratory patterns at 80 °C and at 100 °C, so "the overheating temperature of washers in the second family of transformers is probably around 90 °C" (p. 1734). In a transformer, CIGRE notes, the same gas formation comes from a hotter spot, because of oil convection and cooling: "gas formation at 90°C in the laboratory will likely be produced by a hot spot of e.g., 130°C in the transformer" (TB 771, App. G.5, p. 63). Applied to the washers, that gives about 130 °C. The authors do not take that step (our inference), and CIGRE warns that laboratory results "should be used only with caution to predict the actual temperature of faults in transformers in service" (TB 443, Cl. 3.2, p. 9). After the washers were removed, the authors infer "a small hotspot in oil … of around 180 °C in the underlying electrical contact", which they call "not a concern according to [2]", [2] being TB 771 (p. 1734). The paper explains the change of pattern, not the change of amount (ours): "At lower temperatures (below 120 °C) mainly hydrogen is generated, at higher temperatures (150 to 200 °C) saturated hydrocarbns [sic] are the dominating gases" (p. 1729).
Figure 2, row by row (Buchacz, Buchacz & Duval 2021; sister-unit range from the paper's Fig. 5 table):
| Year | Unit 2-T2 and its family | p. |
|---|---|---|
| 2011 | Gassing reported in all six 115 kV / 63 MVA units | 1730 |
| 2014 | 2-T2's oil changed to a different uninhibited oil | 1730 |
| 2016 | 2-T2: H₂ 11 150 ppm, same pattern as its sister units on the original oil; Pentagon 2 in or near PD. PD tests: very weak in 2-T2, no significant corona PD in the other five | 1731 |
| 2017 | Inspected for the high H₂; galvanised steel washers at an electrical connection removed; back in service | 1731 |
| 2020 | 2-T2: H₂ 5 ppm, zone O. Sister units, listed under "Washers" in the paper's table: 623 to 5 025 ppm. Sister unit 2-T5: very weak PD in phase W, not in the washers | 1731 |
| Inferred | Washers probably around 90 °C; contact around 180 °C after removal; the authors, citing CIGRE TB 771: "not a concern according to [2]" | 1734 |
Reference The washers and water
The authors tie the hydrogen to the galvanised steel washers because it "disappeared when the washers were removed from transformer 2-T2" (p. 1734). They do not discuss hydrogen from galvanised steel and water. IEC 60599 lists that route among other sources of gas: hydrogen "can be produced by reaction of steel and galvanized steel with water, as long as oxygen is available from the oil nearby", and its example of an indication is "hydrogen with the total absence of other hydrocarbon gases" (Cl. 4.4, p. 12). The 2016 sample from 2-T2 also carried 489 ppm of methane and 115 ppm of ethane (Fig. 6 table, p. 1731). CIGRE describes the reaction for oil sampling valves of galvanised steel, which with free water "can produce large quantities of hydrogen at ambient temperature or above", and adds that sampling valves are today made of brass or stainless steel (TB 771, § 2.3, Note 3, p. 15). IEEE C57.104 classes such reactions, "in oil sampling valves of transformers or with tank stell [sic] (rust)", as catalytic fault R, and calls R faults "very rare" (Annex C.2, p. 60). CIGRE's later definition leaves gas "provoked or catalyzed by external factors", electroplated metal surfaces among them, outside stray gassing (TB 927, § 1.5, p. 13); whether galvanised washers fall under that exclusion, CIGRE does not say (ours).
The title's first half is TB 771's reading. CIGRE TB 771 reads stray gases as an indication of abnormal oil temperature somewhere inside the transformer. It writes that "Stray gassing of oil may actually be viewed as a way to detect such abnormal overheating rather than being a nuisance" (App. G.2, p. 61; the paragraph whole).
Reference TB 771 on stray gases as a symptom
The whole paragraph of TB 771, App. G.2: "Although stray gases do not affect the normal operation of transformers, they should not be considered as 'irrelevant' gases that are due only to the chemical instability of oils and unrelated to what is happening in the transformers. They are rather an indication of abnormal oil temperature somewhere inside the transformer (not supposed to exceed ~105°C in transformer loading guides), due to design or operational problems, which may or may not need to be fixed after discussions with the transformer manufacturer. Stray gassing of oil may actually be viewed as a way to detect such abnormal overheating rather than being a nuisance" (App. G.2, p. 61).
In our reading of TB 771 and TB 927, stray gassing is a conclusion the steps in What we recommend can reach, not a reason to skip them (App. G.2, p. 61; § 1.1, p. 9).
IEEE C57.104's main text carries both readings (the IEEE note).
Is stray gassing harmful?
Among the cases reported to CIGRE's working group, no failure due to stray gassing was reported: "No case of failure due to faults S have been reported to the WG at any hydrogen level, high or low" (TB 771, § 3.2, p. 17). IEC 60296's wording is an absence of proof, and it covers gas that is stray gassing only: "In practice, gas due to stray gassing only has not been proven to be harmful to the equipment" (IEC 60296, Cl. 6.19, p. 20). CIGRE's argument on harm turns on temperature and location. TB 771 argues that the temperature at which stray gassing occurs, 120 to 200 °C, "is not high enough to damage the electrical insulating properties of oil" (TB 771, App. G.2, p. 61). TB 771 adds that "Adjacent paper insulation will be at a much lower temperature and even less affected" (App. G.2, p. 61). In our reading, that holds only when the heating stays in the oil away from paper: IEC 60599 puts significant rates of paper polymer chain scission at temperatures higher than 105 °C (IEC 60599, Cl. 4.2, p. 12). Our view: none of these statements is a finding about a given unit.
The corona-PD cases reported to CIGRE, and how CIGRE rates them, are in How much gas: the documented cases.
CIGRE's worked example of a fault S is a sealed power transformer with coated paper, with 48 273 ppm of hydrogen, 3 452 of ethane and 7 of acetylene. Triangle 1 gave T1, Triangle 4 and Pentagon 2 gave S, and the inspection found overheating of pressboard between windings, which CIGRE calls consistent with the gas formation observed in Triangle 4 in zone S (TB 771, § 3.2, p. 17; Table 3.2, p. 18; the example).
IEEE C57.104-2019 says transformers in DGA Status 2 "are considered as possibly suspicious and warrant additional investigation". Where the fault diagnosis then reveals partial discharge, a low-temperature fault or stray gassing, IEEE says the issue "would be treated as a less urgent issue, but still may affect future life of the insulation system". IEEE C57.104 also lists stray gassing among the "more benign conditions", and its informative Annex F, an alternative severity method, excludes suspected stray gassing "from consideration for the detection, assessment, and identification of faults" (IEEE C57.104, Cl. 6.1.2.2, p. 36; Cl. 6.1 a), p. 32; Annex F, p. 81; the IEEE note). In our judgement, Annex F is the nearest the sources come, in print, to treating the gas as noise.
Reference IEEE C57.104: Cl. 5.3.2 and Annex F
IEEE C57.104-2019 says transformers in DGA Status 2, a status set by gas levels, deltas and rates (Fig. 2, p. 34), "are considered as possibly suspicious and warrant additional investigation". Where the fault diagnosis then reveals partial discharge, a low-temperature fault or stray gassing, the issue "would be treated as a less urgent issue, but still may affect future life of the insulation system" (Cl. 6.1.2.2, p. 36). The same guide describes stray gassing as gas formed "at normal service temperatures, rated loading or from material interaction (such as some metal passivators), even if no fault is present" (Cl. 4.1, p. 19). Among the limitations of DGA it notes: "Unusual causes of gas formation can misdirect DGA diagnosis. For example, when a pattern consistent with 'stray gassing' is observed, the possibility of that explanation should be carefully considered before further action is taken" (Cl. 1, p. 12). Its informative Annex F, an alternative method for judging fault severity, goes furthest: gas production "that is suspected to be stray gassing is to be excluded from consideration for the detection, assessment, and identification of faults" (p. 81).
In its screening protocol C57.104 attaches the caveat to the low-temperature fault only: "this would be treated as a less urgent issue, however a low temperature fault (T1) may affect the future life of the insulation system" (Cl. 5.3.2, p. 29). In Cl. 6.1.2.2 it covers stray gassing too (p. 36). Where significant ethane stray gassing is suspected, Annex F allows NEI3oil, the normalised energy intensity NEIoil (Eq. F.1) recalculated with the ethane concentration set to zero, in its place (text after Eq. F.2, p. 82). That stops stray-gassing ethane inflating an energy index; it does not close the temperature question.
When to test for stray gassing, and why no gas level settles it
No gas value, by itself, classifies a unit; the documented cases, each with what its source says, are in How much gas: the documented cases.
Reference How much gas: the documented cases
None of these values classifies a unit. At thousands to tens of thousands of ppm of hydrogen, inspections found a source in the unit (rows 6 and 8); in the same range, cases of faults S were reported to CIGRE's working group without failure (row 7). For the cases at tens to hundreds of ppm (rows 1 to 3), the sources report no inspection.
| Source and case | Gas carried | What the source says |
|---|---|---|
| 1. TB 927, case 2.5 and Table 9, pp. 29–30. Network transformer, 25 MVA, 20 kV, built 2020, uninhibited oil; sample 2021 | H₂ 166, CH₄ 22, C₂H₆ 132 µl/l | Degassed, the oil gassed in the test; "The results demonstrate the strong Stray Gassing tendency of the oil" |
| 2. TB 927, case 2.7, p. 30; Table 10, p. 31. Step-up transformer, 780 MVA, 420 kV, built 1985, uninhibited oil; 2009, before reclaiming | H₂ 45, CH₄ 96, C₂H₆ 205, C₂H₄ 30 ppm | Two years after regeneration and inhibition: C₂H₆ 20, CH₄ 8 ppm; "Regeneration with fuller's earth with consequent inhibiting removes the source of gassing" |
| 3. IEC 63585, Annex C.6, Tables C.20–C.21 and C.6.3–C.6.4, pp. 37–39. Power transformer, 200 MVA, 420 kV, soybean-based natural ester; Dec 2018 to Oct 2021 | H₂ 42 to 330, C₂H₆ 208 to 340 µl/l; C₂H₂ 0.5 and 0.3 µl/l in the first two samples, then 0 | Not inspected. "they relate to stray gassing"; "No inspection, since normal service, no fault" |
| 4. TB 296, Table 16 and Notes, p. 14; § 8.2, p. 19. TB 296's calculation, eight oils, one year in service | H₂ 10 to 520 ppm at a 98 °C hottest spot; 50 to 3 100 at 140 °C; "rough estimates only", possibly ×2 for the top oil | Unless "a very strongly stray gassing oil is used or operation is largely above nominal load", stray gassing "in general will not interfere with DGA diagnoses in service, as initially assumed". CIGRE's 2024 brochure judges that tests at 120 °C and above "strongly contradict real results" (TB 927, § 1.1, p. 9) |
| 5. TB 771, § 3.2, Table 3.1 and note, p. 17. TB 771's hydrogen levels for faults S, power transformers | "Typical" 460; Intermediate 1: 800; Intermediate 2: 1 100 ppm; calculated pre-failure value 2 840 ppm | "a PF value much higher than this calculated PF value could probably be used" |
| 6. Buchacz et al. 2021, Figs. 5–6 tables, p. 1731; p. 1734. Washer family, six 115 kV, 63 MVA units | H₂ 2 385 to 11 150 ppm (2016); sister units 623 to 5 025 ppm (2020) | High H₂ "was due to the galvanized steel washers used"; the authors attribute the gas to stray gassing of oil "between 90 °C and 180 °C depending on the individual units", and conclude: "Such SG of oil is not a concern for the safe operation of these transformers" |
| 7. TB 771, § 3.2, note, p. 17. Cases of faults S reported to CIGRE's working group | H₂ 8 400 to 55 000 ppm | Reported to the WG: "no failure" |
| 8. TB 771, § 3.2 and Table 3.2, pp. 17–18. CIGRE's worked example of a fault S: sealed power transformer, coated paper | H₂ 48 273, CH₄ 11 485, C₂H₆ 3 452, C₂H₄ 8, C₂H₂ 7 ppm; Triangle 4 S, Pentagon 2 S | "Overheating of pressboard between windings found by inspection, consistent with gas formation observed in Triangle 4 above in zone S." |
For comparison, IEC 60599's "90 % typical" hydrogen values for power transformers, from about 25 networks, run from 50 µl/l in one network to 150 µl/l in another (Table A.2 and A.2.4, p. 26). IEC states that these values "are not limit values" (A.1, p. 24). For values above them, the same annex says that "the only action recommended in this document is to increase the frequency of DGA analyses" (A.1, p. 24); the procedure of Cl. 9 adds further steps once a fault has been identified (the ladder). Its higher values for wind turbine transformers come with the caveat quoted under Against partial discharge.
For esters, IEC 63585, quoting IEC 60599, says that percentile values "shall not be used to ascertain whether or not a fault exists within the equipment" (IEC 63585, Cl. 5.2, p. 16). Its informative database gives 90th percentiles of 117 µl/l of hydrogen and 332 of ethane for soybean-based natural ester (8 000 records), 27 and 4.5 for high-oleic sunflower-based natural ester (3 500 records), and 62 and 37 for synthetic esters (7 700 records); the 95th and 98th are in the same tables (Annex B, Tables B.2–B.3, p. 25; Table B.4, p. 26).
Row 3 is IEC 63585's example C.6. The unit was not inspected, so the verdict that follows was not checked by an inspection (ours). Neither the standard's interpretation scheme nor its two-gas ratios indicated a deficiency (Table C.22, p. 38; C.6.4, p. 39). Row 3's ethane is Table C.21's; for 28 May 2019 it prints 255 µl/l, where the Pentagon table prints 268 (Table C.21, p. 37; Table C.23, p. 39). Table C.21 also prints 0.5 and 0.3 µl/l of acetylene in the first two samples and 0 in the eleven after; the Pentagon table prints 0 throughout (Table C.21, p. 37; Table C.23, p. 39). The standard's scheme tests acetylene against its 90th percentile, not against detection (Table C.22, step 1.1, p. 38); step 1 of What we recommend, which gates on acetylene detected and confirmed, is stricter (ours). The standard records that the gases "relate to stray gassing" and gives as its verdict "No inspection, since normal service, no fault" (Annex C.6, Tables C.20–C.21 and C.6.3–C.6.4, pp. 37–39).
TB 296's 2006 conclusion in row 4 rests on results at 120 °C, extrapolated to other temperatures, and CIGRE's 2024 brochure judges tests at that temperature to contradict real results (TB 296, § 3.4, p. 13; § 8.2, p. 19; TB 927, § 1.1, p. 9). Applying that judgement to TB 296's Table 16 is our reading.
Among the cases reported to CIGRE's working group, no failure was reported for more than 15 stray-gassing cases with hydrogen between 8 400 and 55 000 ppm (TB 771, § 3.2, p. 17), nor for more than 30 corona-PD cases between 5 000 and 33 000 ppm, "particularly in wind farm transformers and bushings" (§ 3.3, p. 19). In our reading, CIGRE's next words are about damage and failure, not about cause. As long as corona PD does not evolve into the sparking type, CIGRE calls it, like stray gassing, of "relatively little concern" (§ 3.2.2, p. 18; § 3.3, p. 19), and of no significant effect on the operation of transformers "in the short term" (App. D.1, p. 55).
Row 8: a zone S result can sit on overheated solid insulation (ours).
Reasons to test the oil; none of them shows that the gas is stray gassing.
- Hydrogen, methane or ethane up, alone or together.
- No acetylene. None of the bench tests cited here reports acetylene: CIGRE reports that acetylene was never observed in its round robin, and IEC 63585 says none was generated (TB 927, § 1.7.1, p. 16; IEC 63585, Cl. 4.1.4, p. 13). TB 771's worked example of a fault S prints 7 ppm of acetylene, and there the inspection found overheated pressboard (TB 771, § 3.2, p. 17; Table 3.2, p. 18; the example). For a service sample the conclusion is ours: stray gassing does not explain acetylene. The other datasets are in Acetylene in the datasets.
- Ethylene small and not rising. CIGRE reports stray-gassing ethylene only in a very few occurrences, each with a named cause (TB 771, App. G.4, p. 62); a steady rise that none of them explains points, in our reading, to a thermal fault.
- Zone S, or close to it. In mineral oil, Triangle 4 or Pentagon 1 or 2 puts the point in zone S, the stray-gassing zone of the Duval diagrams. Or it lies very close to the S/PD boundary, where CIGRE TB 771:2019 says stray gas formed with some oils at 120 °C sometimes falls (App. G.2, p. 61). IEEE C57.104 says Triangle 4 "should be used only in case of faults identified first as faults PD, T1 or T2 in Triangle 1" (Annex D.4, note b), p. 66).
- A shape over time. The gas levels off, or oxygen falls as it rises (what each sign settles).
- A new, refilled or repaired unit (below).
Reference Acetylene in the datasets
IEC 63585 states of the CIGRE round robin on synthetic ester, soybean-based natural ester and uninhibited mineral oil, at 105 °C for 48 h, that no acetylene was generated under those test conditions (IEC 63585:2026, Cl. 4.1.4, p. 13). Hanson's ester liquids print 0 (Table III, p. 140), and CIGRE's 2020 network transformer prints less than 1 µl/l before and after its test (TB 927, Table 9, p. 29). The laboratory method's own rule, "Acetylene should not be detected. If acetylene is detected, then the results should be considered suspect and the process reviewed" (ASTM D7150-13, Cl. 7.12, p. 4), governs the laboratory run.
Carbon monoxide does not discriminate (why). Check your own report in the Duval Triangle tool or the Duval Pentagon tool.
A new, refilled or repaired unit
Gas in a new, refilled or repaired unit has more than one possible source, a fault among them, and which one applies has to be shown on the unit (IEC 60599, Cl. 4.4, p. 12; IEEE C57.104, Cl. 5.3.1, p. 28). CIGRE has found stray gassing "in both new and aged transformers", among them the 2020 network transformer of row 1 of the documented cases (TB 927, § 1.1, p. 9; § 2.5, p. 29; commissioning and the other sources).
Reference New and repaired units: acetylene and residual gas
In its guidance for ester-filled equipment, IEC 63585 notes that during commissioning "Transient effects can take place … leading to high gas generation but not necessarily to a fault in the equipment". In the next sentence it adds: "Conversely, major failures have been observed in some cases at very low gas generation" (Cl. 5.1, p. 15).
In a 25 MVA network transformer built in 2020 the oil gassed shortly after commissioning, and the degassed sample gassed again in the laboratory test (TB 927, § 2.5 and Table 9, p. 29). IEC 60599 calls its other sources of gas very unusual, but lists acetylene among the gases that new stainless steel can absorb during manufacture, or that welding can produce, and that are "released slowly into the oil" (Cl. 4.4, p. 12).
For new and repaired units IEEE C57.104 names a further explanation, "residual gas from an earlier fault diffusing into the insulating liquid from the paper insulation in a repaired transformer". It counts insulating-liquid processing and repairs among the events that "reset" a unit's DGA history (Cl. 5.3.1, p. 28). CIGRE found gas held in paper still coming out "sometimes quite a long time (8 years) after re-energization" (TB 296, § 6, p. 17). IEEE notes that "typically in an initial verification context, gas level norms lower than Table 1 are used" (Cl. 5.3.1, p. 29).
IEC 60599 lists other sources of gas, among them steel and galvanised steel reacting with water, which has produced large quantities of hydrogen "in some transformers that had never been energized". It calls such occurrences very unusual (Cl. 4.4, p. 12; the list).
What the DGA can and cannot tell you
Against partial discharge
On paper, the CH₄/H₂ ratio separates the two in TB 296: corona partial discharge sits at 0.02 to 0.14, while stray gassing sits at 0.15 to 1 at 120 °C or above 0.4 at 200 °C (TB 296, Table 18 and § 3.5, p. 15). In the field, three of the four TB 771 cases that Triangle 4 places in zone S (cases C, A and E) sit at 0.083 to 0.100: inside the corona band, beside partial-discharge case B (TB 771, Table 3.3, p. 19; ratios our calculation; why they part ways).
The ratio and Triangle 4 part ways over ethane, which the CH₄/H₂ ratio does not use. Cases C, A and E carry 500, 200 and 400 ppm of ethane, 1.8 to 5.7 % of Triangle 4's three gases. IEEE draws Triangle 4's PD zone at ethane below 1 % (with methane from 2 to below 15 %), so they fall in S. Case B carries none and falls in PD (TB 771, Table 3.3, p. 19; IEEE C57.104, Table D.3, p. 65; percentages ours).
Reference Figure 4: the CH₄/H₂ bands and the five field cases
TB 771 calls stray gassing and partial discharge "sometimes difficult to distinguish" (§ 3.3, p. 18). The bands come from TB 296 Table 18, which the brochure credits to M. Duval of Hydro-Québec, listed in its key among the authors of unpublished data or specific contributions, for gases formed in service (Table 18, p. 15; key, p. 20). Table 18 also has a band for catalytic reactions, below 0.02, and TB 296 says stray gassing can be differentiated from corona PDs or catalytic decomposition by the CH₄/H₂ ratio of gases formed in service (TB 296, Table 18 and § 3.5, p. 15). The two stray-gassing bands share 0.4 to 1, so the ratio cannot separate the two temperatures.
The bands contradict the folk rule, which says stray gassing shows a low CH₄/H₂ and is therefore mistaken for partial discharge. The folk rule has support: after the first 16 hours at 120 °C, at least five of the nine oils in TB 296's own Table 13 give a CH₄/H₂ below 0.15; a sixth prints its methane as 0, which TB 296 uses for anything below 2 ppm, so its ratio cannot be placed either side of 0.15 (Table 13, p. 12; Annex C, Table C1 note, p. 27; our arithmetic). CIGRE's field cases side with it too.
TB 771 lists five cases with their gas concentrations and two Duval classifications, but no ratio column. The ratios and the ethane shares below are our arithmetic on the values it lists.
| Case | H₂ / CH₄ (ppm) · ratio | C₂H₆ (ppm) | Triangle 4 · Pentagon 2 |
|---|---|---|---|
| C | 12 000 / 1 000 · 0.083 | 500 | S · S |
| A (2011) | 10 000 / 1 000 · 0.100 | 200 | S · PD |
| E | 6 000 / 600 · 0.100 | 400 | S · S |
| B | 15 000 / 1 500 · 0.100 | 0 | PD · PD |
| D | 300 / 150 · 0.500 | 0 | S · C |
Ratio = CH₄/H₂. S = stray gassing, PD = partial discharge, C = possible carbonization of paper (IEEE C57.104, Table C.1, p. 59; Table C.2, p. 60). TB 771, Table 3.3 and notes, p. 19. Acetylene is 0 in every row. Our arithmetic: A 200/11 200 = 1.8 %, C 500/13 500 = 3.7 %, E 400/7 000 = 5.7 %, B 0 %; methane shares A 8.9 %, C 7.4 %, E 8.6 %, B 9.1 %.
- Reading the cases. Cases C, A and E, which Triangle 4 places in zone S, sit at 0.083 to 0.100: below the stray-gassing floor, inside the corona band. Case D, at 0.500, falls where the two stray-gassing bands overlap. So band and Triangle 4 agree on two cases of five, B and D. In case A, Pentagon 2 says PD, as the ratio does. For case D, TB 771's note sides with Pentagon 2. Its notes put the S or PD activity on metal in the oil; in case D a small layer of paper between metal parts explains the small fault C (Table 3.3 and notes, p. 19).
- Cases D and A in detail. Case D carries 75 ppm of ethylene, and its note reads "a small layer of paper between metal parts, hence the small fault C". Case A also has a 2012 row: hydrogen 0, methane 2 000 and ethane 700 ppm, classified C/O by Triangle 4 and O by Pentagon 2, and the note reads "in A-2012, fault O was in windings"; with no hydrogen it has no ratio (TB 771, Table 3.3 and notes, p. 19).
- IEC 60599 and IEC 63585. IEC 60599 Table 1, the interpretation table most readers work from, carries six fault cases and no stray-gassing row. Its partial-discharge row is a CH₄/H₂ below 0.1 (below 0.2 in instrument transformers and below 0.07 in bushings, NOTE 3), and CIGRE's field cases sit on its edge (p. 14). Its NOTE 4 says that gas decomposition patterns similar to partial discharges have been reported as a result of stray gassing of oil (IEC 60599:2022, p. 14). Where Table 1 gives no diagnosis, the standard allows the simplified scheme of Table 2 for at least a rough distinction; its partial-discharge line is CH₄/H₂ below 0.2, and cases A, B, C and E all fall inside it (IEC 60599:2022, Table 2, p. 14). In esters, IEC 63585 brings stray gassing into the CH₄/H₂ reading only in a NOTE to its partial-discharge clause. With clean sampling, partial discharge usually gives values below 0.1 or 0.2, and a poor sampling point, especially on wind and traction units, lets hydrogen escape and pushes the ratio towards 1. The NOTE adds that a ratio of 0.1 to 1 can be also due to a low-temperature fault or stray gassing (Cl. 5.3.2, p. 18). For esters IEC 63585 also notes that in partial discharge "the ratio methane/ethane (due to the lower volatility of both in comparison to hydrogen) is more stable than the ratio of hydrogen/methane and has usual values of 4 to 6" (Cl. 5.3.2, p. 18). In a natural ester that makes ethane by itself (Cl. 5.3.5, p. 19), that ethane lowers the ratio whatever the PD does, so the check says less there than in a synthetic ester (ours).
- Why the question matters. The field paper's authors write that hydrogen formed by stray gassing "is often mistakenly attributed to corona PDs, sending false alarms of electrical faults to maintenance engineers". Their remedy is to run the tests on "the oil sampled from transformer in concern" (Buchacz et al. 2021, p. 1729).
- Liquid not named. TB 771's high-hydrogen stray-gassing and corona-PD cases do not name the liquid (§ 3.2–3.3, pp. 17–19).
For wind turbine transformers, IEC 60599 says its statistical hydrogen values "could not be inherently attributable to fault absence", and that experience worldwide "is not sufficiently large, yet, to define which statistical values can be considered as fault-free" (IEC 60599:2022, Table A.5, footnote c, p. 28).
In IEC 63585's wind-farm example, a 3.3 MVA synthetic-ester unit was inspected after its pressure relief device operated. The standard's interpretation scheme and the Duval triangle for synthetic ester indicated partial discharge; the Duval pentagon for synthetic ester gave S. The PD measurement showed PD activity, and the internal inspection found X-wax on the surface of the insulation. The sample had been taken from the nitrogen pressure device and not according to IEC 60475, which the standard says "can have led to a considerable loss of hydrogen". Its comment is that under the same conditions, different interpretation schemes can lead to different assessments (IEC 63585:2026, Annex C.2, pp. 27–29).
CIGRE's account of the high hydrogen, with the cause it gives, is in CIGRE on wind-farm transformers.
Reference CIGRE on wind-farm transformers
IEC 60599 reports CIGRE's finding that faults in wind turbine transformers are "mostly of the corona PD and T1 types, sometimes T3" (IEC 60599:2022, A.3.2, NOTE, p. 28). In an appendix whose values come "from databases outside of the WG" (App. D, p. 55), CIGRE writes that wind-farm transformers are "well-known to generate high to very high levels of hydrogen due to stray gassing of oil S and partial discharges of the corona-type PD (up to 55,000 ppm in some cases)". It gives the cause with the observation: "This high gas formation, without failure in most cases, is due to the transformers being of the Padmount-or distribution-type used, which were not designed for the highly variable loads they are subjected to, creating harmonics and overheating. Also, due to tank constraints, they cannot be oil-impregnated under vacuum, resulting in the formation of voids in paper and partial discharges of the corona-type PD." CIGRE reports a belief and answers it: "It is sometimes believed that very high levels of hydrogen (several thousand or tens of thousands of ppm) in transformers cannot be due to stray gassing (overheating) of oil, but only to partial discharges of the corona-type PD"; against it, "numerous such cases were reported to the WG, which were not due to partial discharges of the corona-type PD (no PD signal during PD tests on the transformers), but indeed to stray gassing of oil only". As long as they do not evolve into the sparking type, CIGRE adds, "partial discharges of the corona-type PD do not significantly affect the operation of transformers in the short term"; CIGRE's marker for that change is acetylene: if they "evolve into more dangerous partial discharges of the sparking-type, they will immediately initiate the formation of acetylene, indicating the fault progression" (TB 771, App. D.1, p. 55). TB 771's App. G.2 places the very high hydrogen levels "particularly in wind farm transformers and bushings (see APPENDIXES D.1. and D.2.) but also in power transformers" (p. 61). IEC 60599 prints CIGRE's wind-turbine values with the caveat that they "could not be inherently attributable to fault absence" (Table A.5, footnotes a and c, p. 28); of the same units TB 771 says the hydrogen levels of its Table 3.1 for faults S "can therefore be significantly increased" (§ 3.2.1, p. 18).
Near the S/PD boundary. TB 771 recommends a laboratory stray-gassing test on oil from the transformer, and adds that a PD test on the whole transformer "may also confirm the absence of partial discharges of the corona-type PD" (App. G.2, p. 61; the checklist).
Against a thermal fault
The DGA alone may not settle it: telling stray gassing from a T1 or T2 thermal fault, TB 296 says, is more difficult. TB 927 asks whether IEC 60599's T1 "is really connected with a fault or with the stray gassing" (TB 296, § 3.5, p. 15; TB 927, § 1.1, p. 9; TB 296's rough check).
Reference TB 296's rough check and the pattern comparison
Two of the questions that remain open when the oil gasses in the test (step 9):
- Whether anything ran hotter than the temperatures usual in service. TB 296 offers a rough check: test the oil at the unit's expected average hottest-spot temperature and scale the result to the most the oil can add in service. If the gas in service is above that level, "a thermal fault is more likely than stray gassing"; below it, "it will not be possible to differentiate between stray gassing and thermal faults T1 / T2" (§ 3.5, p. 15). TB 296 calls its own scaled values "rough estimates only", which "may have to be multiplied by a factor of about 2" for the top oil (Table 16, Notes 1–2, p. 14). CIGRE wrote in 2024 that there is no criterion for comparing gas in service with the oil's stray gassing (TB 927, § 1.4, p. 13).
- How the test compares with the service DGA. In one CIGRE case "hydrogen, methane and ethane were produced in similar ratios as in the transformer" (TB 927, case 2.4, p. 29). A different pattern at 105 °C does not rule the oil out. In the field paper one unit's oil led with hydrogen in five of the six 105 °C runs (under nitrogen with copper, ethane 94 ppm against hydrogen 84) and with ethane in service, and the authors matched the service pattern at a higher test temperature (Buchacz et al. 2021, Fig. 3 and Fig. 10 tables, pp. 1730, 1733; p. 1734).
TB 296's procedure, step by step: (1) estimate the expected average hottest-spot temperature of the oil in the unit. (2) Run a laboratory stray-gassing test on the oil from the unit at that temperature, not at the 105 °C of an IEC 60296 certificate (the contrast is ours). (3) Scale the result to the maximum the oil could contribute in service (CIGRE TB 296:2006, § 3.5, p. 15). TB 296's Table 16 is extrapolated from 120 °C results: "Values for the other oils were extrapolated by drawing curves parallel to these experimental curves from the value available for these oils at 120°C" (§ 3.4, p. 13). The procedure describes what the laboratory does; it is not an instruction to the operator.
When the oil gasses in the test. The test does not show that the oil made all of the gas in service, or at what temperature, and whether anything in the unit ran hotter than usual service temperatures remains open. Under IEC 60296's definition the answer can be no: it defines stray gassing at "temperatures considered usual for normal operating conditions" (Cl. 6.19, p. 20). CIGRE reports T1-like readings in transformers "operating far below its nominal rating", in units that "exhibited no deficiencies based on electrical tests" (TB 927, § 1.1, p. 9). TB 296 calculates a year's stray-gassing hydrogen even at an 85 °C hottest spot, values it says "should be viewed as rough estimates only" (Table 16 and Note 1, p. 14).
Ethylene. The laboratory test makes some. In mineral oil, CIGRE reports stray-gassing ethylene in a very few occurrences, each with a named cause (TB 771, App. G.4, p. 62): decomposition of some passivator additives; reclamation on aluminosilicates or bauxite to remove corrosive sulphur; sometimes, reclamation on Fuller's earth or bauxite under high oxygen content; some older solvent-based oils no longer in use. If none fits the unit's history and the ethylene keeps rising, we read it as a thermal fault. In a natural ester, IEC 63585 reads the trend of C₂H₄/C₂H₆: a significant rise in the ratio during operation "could suggest the possibility of an incipient high-temperature thermal fault, even if C₂H₄/C₂H₆ does not reach values > 1" (IEC 63585, Cl. 5.3.5, p. 19; ethylene in the laboratory test).
Reference Ethylene in the laboratory test
- The laboratory test makes some ethylene: up to 17 ppm in TB 296's full 120 °C results, where a dash means less than 2 ppm, not zero (Annex C, Table C1, pp. 26–27), and 37 to 40 ppm after 24 hours at 200 °C (Table C2, p. 28).
- The 17 ppm in TB 296's 120 °C results comes from an oil the table lists as one year old; the three oils TB 296 tested at both temperatures print 4 ppm or less in every 120 °C run (Annex C, Tables C1 and C2, pp. 26–28).
- A later CIGRE test went higher: a less refined commercial oil meeting IEC 60296 for standard oils, held 16 hours at 120 °C in glass syringes, gave 41 ppm, which the brochure calls unexpected (CIGRE TB 771:2019, App. G.5 and App. Table G.1, pp. 62–63).
- Another laboratory of CIGRE's working group, using syringes and sealable glass ampoules, the containers TB 771 recommends instead of screw-capped vials (App. G.3, p. 62), found ethylene at 150 and 200 °C: 37 and 72 ppm in oil without BHT antioxidant, 19 and 90 ppm with 0.3 % BHT. TB 771 reads the patterns as moving with temperature from zone O (without BHT) or zone S (with BHT) to zone T2 (App. G.5, p. 63; App. Table G.2, p. 64).
- What the oil was sealed in matters. Vial screw caps and septa can themselves produce ethylene above 90 °C, so TB 771's list of reasons names screw-capped vials too, an artefact of the laboratory test, not of the transformer (App. G.3 and G.4, p. 62). The field paper's 2016 tests were all made in vials (p. 1730): they print up to 213 ppm of ethylene at 150 °C (Fig. 12 table, 150 °C vial rows, no duration printed) and up to 154 ppm in the 72-hour runs at 150 °C (Fig. 13 table) (Buchacz et al. 2021, p. 1733). The paper does not discuss whether the vials contributed (ours).
Trend. IEC 60296 says stray gassing usually levels off with time, and for natural esters IEC 63585 says the gas concentration typically tends to stabilise (IEC 60296, Cl. 6.19, p. 20; IEC 63585, Cl. 4.1.2, p. 11). A plateau is the textbook shape, not the only one: some of CIGRE's service cases kept climbing (the cases that kept climbing).
Reference Trend: what the cases show
On the bench the rate falls after the first 16 hours by a factor of ~2 to 12 depending on the oil (TB 296, § 3.2, p. 12). CIGRE reports that gas may appear down to 40–45 °C if a sufficient testing duration is achieved (TB 927, § 1.4, p. 12). Do not convert hours in the laboratory test into service weeks: TB 771's one such comparison, the same amounts after 1 week at 120 °C and after 30 weeks at 40 °C, carries the note "This, however, has not been reconfirmed nor observed in actual transformers" (App. G.3, p. 62). IEEE C57.155 reports that ester ethane has been observed in service to stabilise or level off over time (Cl. 4.1.1, p. 5). The TB 927 case 2.4 unit's hydrogen rose steadily from 2005 to 2016, and its ethane and methane rose until 2015 (case 2.4 and Fig. 12, p. 28). Case 2.6 is 53 free-breathing units whose ethane and methane kept climbing, with reduced oxygen content (p. 30). IEC 63585 adds that, in natural esters, continued ethane increase can indicate the presence of air in the transformer (Cl. 4.1.2, p. 11).
Oxygen. Falling oxygen fits stray gassing and the other low-temperature faults alike (TB 927, case 2.7, p. 30; TB 771, App. F.3, p. 59; what the sources say).
Reference Oxygen: what else the sources say
Oxygen speeds stray gassing (IEC 60296, Cl. 6.19, p. 20). Where CIGRE found stray gassing, it wrote: "The lower than expected oxygen content in the oil suggested an on-going oxidation" (TB 927, § 1.1, p. 9). CIGRE reports that "Very often stray gassing behaviour is accompanied with oxygen depression" (TB 927, case 2.7, p. 30). Ethane and methane rise faster as oxygen is depleted, which CIGRE reads as an indication that they "can be a consequence of oxidation processes" (TB 927, § 2, p. 24). Falling oxygen is not specific to stray gassing. TB 771 reads a decrease in oxygen as oil oxidation "because of oil overheating, which may be normal or abnormal" (App. F.1, p. 59). In TB 771's database more of all the low-temperature faults and stresses, T1, O, S, C and T2, occur at low oxygen/nitrogen ratios. "It is not clear, however, whether low temperature faults or stresses are the consequence or the cause of the low oxygen/nitrogen ratios" (App. F.3, p. 59). IEEE C57.104 says decreasing O₂/N₂ values "indicate overheating and oxidation of mineral oil and can be used to confirm thermal faults" (Annex D.9.1, p. 69). For esters, among the correlations to trend, IEC 63585 gives "the consumption of oxygen and the production of ethane" as an example of "thermo-oxidative gassing, no serious fault condition likely" (Cl. 5.5, p. 20). A rise in oxygen is not that shape: in one unit it followed reclamation (TB 927, Table 10, p. 31; the case).
The 780 MVA unit had uninhibited oil, reclaimed on fuller's earth and then inhibited. Two years later oxygen had risen from 6 150 to 24 850 ppm while ethane fell from 205 to 20 and methane from 96 to 8 (TB 927, case 2.7, p. 30; Table 10, p. 31): the rise in oxygen followed the reclamation.
Reference Esters and oxygen
Air promotes ester stray gassing: IEC 63585 says ethane and hydrogen develop especially in the presence of air (Cl. 4.1.2, p. 11). Air makes more gas than nitrogen "in the majority of cases" (TB 927, § 1.4, p. 13). In CIGRE's round robin, the one natural ester tested, soybean-based, kept its ethane high under nitrogen as well as under air at 105 °C for 48 h (TB 927, Fig. 8, p. 22; IEC 63585, Cl. 4.1.4, Fig. 5 b), p. 14). Other natural esters can behave differently (Cl. 4.1.4, p. 13). IEC 63585 puts the differences between natural esters down to oxidation, "most probably due to oxidation processes" (Cl. 4.1.4, p. 14), while its own figure shows the soybean ester's ethane high under nitrogen too (Fig. 5 b), p. 14); the standard does not reconcile the two (ours). Neither figure behind the round-robin result labels its bars (TB 927, Fig. 8, p. 22; IEC 63585, Fig. 5 b), p. 14), so it gives a direction, not a number.
What each sign settles. A plateau and falling oxygen both fit stray gassing. Neither proves it, and their absence rules out neither. Returning gas proves neither a fault nor stray gassing: it shows that something is still producing gas, or that gas held in the paper is coming out (TB 296, § 6, pp. 17–18).
The Duval zones
An ester S result is read with caution: CIGRE says the Pentagon 3 S zones are at present based mostly on pyrolysis tests. IEC 63585 finds "not enough consolidated evidence that those faults can be identified in esters based on real cases" (TB 771, App. G.6, p. 65; IEC 63585, Cl. 5.6, p. 21; which Duval tool for which liquid).
Reference Which Duval tool for which liquid
- Mineral oil. Zone S in Triangle 4, Pentagon 1 and Pentagon 2. Triangle 4 only for a sample that Triangle 1 has first placed in PD, T1 or T2 (IEEE C57.104, Annex D.4, note b), p. 66). Pentagon 2 keeps Pentagon 1's electrical zones and splits the thermal ones into S, O, C and T3-H. IEEE says it "should be used", with Triangle 4 or 5, where those sub-types are of interest, and that it gives more information on a thermal fault Pentagon 1 has found (Annex D.5, p. 67; Annex D.7, p. 68; also TB 771, App. H.3–H.4, p. 69). Our Duval Pentagon tool plots any sample in Pentagon 2.
- FR3. Zone S in Triangle 6 and Pentagon 3. Triangle 6 once Triangle 3 has returned PD, T1 or T2 (the gate our Duval Triangle tool applies).
- Rapeseed ester. Pentagon 3 first: CIGRE TB 443's Triangle 3 boundaries cover silicone, Midel, FR3 and BioTemp, not rapeseed (TB 443, Table 4, p. 8).
- Other esters. The fluid's own Triangle 3 first, which has no stray-gassing zone; our Duval Pentagon tool has Pentagon 3 for rapeseed, soybean, sunflower and synthetic ester.
The ester S zone changes shape from one ester to the next (TB 771, App. G.6, p. 64). IEC 63585 says the ester triangles and pentagons are documented by analogy with Pentagons 1 and 2 for mineral oils (Cl. 5.6, p. 21). CIGRE names Triangle 4 and Pentagons 1 and 2 as tools that can detect stray gassing (TB 771, App. G.2, p. 61). Below typical values, CIGRE allows the triangles and pentagons for identifying stresses where at least one gas meets IEC's accuracy requirement (±15 % above 10 ppm; ±30 % between 5 and 10 ppm, with the area of uncertainty calculated near a zone boundary); where the laboratory cannot certify that accuracy, it gives IEC's recommendation to use them only above typical values (TB 771, § 2.2, p. 13). See Which Duval Method Should You Use?.
Your liquid sets which gas leads in the test
| Liquid | Leading gas in the test (of H₂, CH₄, C₂H₆) |
|---|---|
| Mineral, uninhibited unused | ethane |
| Mineral, inhibited, triazolic passivator | hydrogen |
| Mineral, inhibited, unused and recycled | none of size; CO leads |
| Mineral, uninhibited recycled | hydrogen |
| Natural ester: soybean, rapeseed, flaxseed | ethane |
| Natural ester: high-oleic sunflower, peanut | hydrogen |
| Synthetic ester | hydrogen |
| Silicone | none at 105 °C; only H₂ at 180–220 °C |
Mineral rows: IEC 60296, air with copper. Ester rows: ASTM D7150 test at 120 °C, oxygen supplied before testing. The tests differ in temperature, duration and copper, so compare the leading gas, never the numbers (values). The leading gas can change with temperature: soybean natural ester already gasses at 90 °C, below the 105 °C of the IEC 60296 test, and leads with hydrogen there (Hanson, Table IV, p. 140). In our reading, a hydrogen-led DGA result on a natural-ester unit therefore neither rules out stray gassing nor points to it rather than to partial discharge; which applies has to be shown on the unit.
Reference What each liquid produces, with values
| Liquid (α-linolenic acid, % as printed) | Leads (of H₂, CH₄, C₂H₆) | H₂ | CH₄ | C₂H₆ |
|---|---|---|---|---|
| IEC 60296 Annex A — 105 °C, 48 h, µl/l | ||||
| Mineral, uninhibited unused (Fig. A.2), air + Cu | ethane | 82.8 | 136.7 | 163.5 |
| Mineral, inhibited, triazolic passivator (Fig. A.3), air, no Cu / Cu | hydrogen | 111.9 / 63.5 | 0.7 / 0.9 | 0.0 / 0.1 |
| Mineral, inhibited, unused and recycled (Fig. A.4), air + Cu | none of size; CO 88.1 | 2.5 | 1.0 | 0.0 |
| Mineral, uninhibited recycled (Fig. A.5), air + Cu | hydrogen | 290.0 | 13.1 | 0.7 |
| ASTM D7150 — 120 °C, oxygen supplied; duration as printed differs (24 h in IEEE C57.155; 164 h in IEC 63585; none in Hanson Table III), ppm | ||||
| Soybean, ~7 % (Hanson III) | ethane | 316 | 10 | 563 |
| High-oleic sunflower, ~0.2 % (Hanson III) | hydrogen | 357 | 21 | 4 |
| Peanut, ~0.2 % (Hanson III) | hydrogen | 282 | 10 | 26 |
| Flaxseed, ~53 % (Hanson III) | ethane | 708 | 17 | 2 371 |
| Rapeseed, approx. 9 % (C57.155 B.1) | ethane | 289 | 60 | 3 694 |
| Synthetic ester (C57.155 B.1) | hydrogen | 175 | 14 | 0 |
| Silicone — 105 / 180–220 / 250 °C | ||||
| Silicone (TB 927, TB 771, TB 443) | no stray gassing / only H₂ / very little | — | — | — |
Mineral rows: bar labels (IEC 60296:2020, Figs. A.2–A.5, pp. 29–32). Ester rows: Hanson et al. 2016, Table III, p. 140, which prints neither temperature nor duration (its text says oxygen and heat were provided "prior to testing as per ASTM D7150", § V, p. 140); rapeseed and synthetic ester from IEEE C57.155-2014, Table B.1, p. 16, which prints the series as a modified 24-hour test with an air sparge. IEC 63585:2026 reprints Hanson's four liquids under a caption of 120 °C for 164 h (Table 1, p. 14), the condition of the unmodified ASTM D7150 Method A (ASTM D7150-13, Cl. 1.5, p. 1). Hanson's Table II gives one liquid, which it does not name, 448 ppm of ethane with the additional oxidation inhibitor and 2 104 without, after an air sparge and 1 day at 120 °C (Table II and § IV, p. 140); its values with the inhibitor equal those of Table IV's soybean oil at 120 °C (ours), and whether it is the liquid of Table III's 563 ppm, Hanson does not say. IEEE C57.155-2014 has been Inactive-Reserved since 27 March 2025, with a revision under development; we cite it only for the data it prints. The current International Standard for ester DGA is IEC 63585:2026. Silicone: CIGRE TB 927:2024, p. 22; TB 771:2019, App. G.6, p. 64; CIGRE TB 443:2010, Cl. 3.2, p. 9. Acetylene is 0 in every ester row. The percentages are α-linolenic acid content as printed, approximate where the source marks them so; IEC 63585:2026 Table 2 reports total poly-unsaturation, a different measure.
Mineral oil: four documented patterns
IEC 60296 prints the round robin of 18 laboratories as four gas patterns: each oil in air and in nitrogen, with and without copper, 48 h at 105 °C (A.1, p. 26; Figs. A.2–A.5, pp. 29–32).
Air with copper is not the worst case for every gas: in A.3 hydrogen is higher without copper (IEC 60296:2020, Fig. A.3, p. 30).
Reference Figure 5: the IEC 60296 round robin
Values in µl/l as labelled on the bars (IEC 60296:2020, Figs. A.2–A.5, pp. 29–32). A.2 is an uninhibited unused oil, A.3 an inhibited unused oil with a triazolic passivator, A.4 inhibited oils, unused and recycled (typical values), and A.5 an uninhibited recycled oil. Bold: the leading gas in air with copper. In A.4 that is carbon monoxide, which is not evaluated and which Figure 5 does not mark.
| Pattern · condition | H₂ | CH₄ | C₂H₆ | CO |
|---|---|---|---|---|
| A.2 · air | 5.3 | 1.9 | 0.8 | 26.0 |
| A.2 · air + Cu | 82.8 | 136.7 | 163.5 | 275.4 |
| A.2 · N₂ | 2.7 | 3.8 | 2.9 | 7.4 |
| A.2 · N₂ + Cu | 3.3 | 17.2 | 8.5 | 26.3 |
| A.3 · air | 111.9 | 0.7 | 0.0 | 26.9 |
| A.3 · air + Cu | 63.5 | 0.9 | 0.1 | 54.4 |
| A.3 · N₂ | 35.1 | 0.7 | 0.5 | 8.3 |
| A.3 · N₂ + Cu | 14.0 | 1.3 | 0.4 | 16.4 |
| A.4 · air | 0.7 | 0.9 | 0.3 | 26.6 |
| A.4 · air + Cu | 2.5 | 1.0 | 0.0 | 88.1 |
| A.4 · N₂ | 1.1 | 1.0 | 0.0 | 7.6 |
| A.4 · N₂ + Cu | 1.1 | 1.2 | 0.0 | 11.7 |
| A.5 · air | 262.4 | 4.6 | 0.2 | 174.4 |
| A.5 · air + Cu | 290.0 | 13.1 | 0.7 | 288.9 |
| A.5 · N₂ | 84.0 | 11.3 | 4.9 | 19.8 |
| A.5 · N₂ + Cu | 23.4 | 17.3 | 7.2 | 37.3 |
IEC 60296 evaluates an oil as delivered, unused or recycled, as "stray gassing" when hydrogen, methane or ethane exceeds 50 µl/l under any tested condition (A.6.2, p. 28); carbon monoxide is not part of the evaluation (A.6.2 NOTE, p. 28).
- A.2 in air with copper also has carbon monoxide above all three hydrocarbons. Under nitrogen with copper methane leads instead, so hydrogen is last either way.
- In the quietest pattern, A.4 in air with copper, carbon monoxide is the only gas of any size (Fig. A.4, p. 31).
- In A.5 in air with copper, carbon monoxide is as high as hydrogen.
- CO and CO₂ respond as well, but IEC leaves them out of the limit: they are more difficult to assess, because in real equipment a certain part of them comes from the solid insulation (A.6.2 NOTE, p. 28). The four figures do not report CO₂ at all.
- Carbon monoxide rises with copper in all eight round-robin pairs, in the oil that passes the 50 µl/l test as well as in the three that fail it (IEC 60296, Figs. A.2–A.5, pp. 29–32; A.6.2, p. 28).
Some 20 mineral oils tested in 2005 "All produced mostly hydrogen at 120°C, and mostly ethane and methane at 200°C" (TB 771, App. G.3, p. 61). CIGRE groups the uninhibited recycled oil with the passivated oil (TB 927, p. 22). Four is not all of them: IEC 60296 says its figures "do not represent a full picture of all the possible stray gassing patterns" (A.8.1, p. 29).
Of the uninhibited unused oil (Fig. A.2), its Sample 1, CIGRE writes: "Sample 1 shows a gas pattern more similar to a T1 faulty condition (ethane is the major hydrocarbon gas); this condition is often observed in service" (TB 927, p. 22).
CIGRE's 2019 brochure says the most important gas formed with faults or stresses S is usually hydrogen. Its 2024 brochure reports service patterns where hydrogen is not the major gas (TB 771, § 3.2, p. 17; TB 927, § 1.5, p. 13).
- Uninhibited unused, in air with copper: methane follows ethane, and hydrogen comes last (Fig. A.2, p. 29).
- Triazolic passivator, a metal-passivator additive: the cleanest hydrogen-only pattern (Fig. A.3, p. 30). Reports on passivators differ (passivators).
- Uninhibited recycled: hydrogen leads in all four conditions (Fig. A.5, p. 32).
Reference Passivators and inhibited oils
Reports on passivators differ. IEC 60599 notes that stray gassing "has been observed in some cases to be enhanced by the presence in oil of a metal passivator or other additives" (Cl. 4.3 NOTE, p. 12). TB 771 lists some passivator additives among the reasons reported for more stray gas, and adds "However, other reports show no significant increases" (App. G.3, p. 62). CIGRE's 2010 brochure found that where the transformer was filled with passivated oil from the beginning, "very little or no stray gassing is observed". Passivator added to oil already in service was followed by increasing hydrogen and carbon monoxide as the passivator content fell (TB 443, Cl. 5.5, p. 20).
In the round robin, the inhibited oils other than the passivated one, unused and recycled, made very little of the three gases: in air with copper 2.5 µl/l of hydrogen, 1.0 of methane and 0.0 of ethane, which IEC prints as "typical values, considering the very low deviation between the tested oils" (IEC 60296, A.8.4 and Fig. A.4, p. 31). CIGRE groups them as liquids with "a very low tendency to stray gassing"; their common characteristic, it says, "seems to be the chemical stability, given by the high grade of refining and the presence of the inhibitors" (TB 927, p. 22). IEC 63585 states of the same round robin that "Inhibited high grade mineral oils … did not show stray gassing in this study" (Cl. 4.1.4, p. 14); the passivated inhibited oil of the round robin did gas (IEC 60296, Fig. A.3, p. 30). TB 771 lists the absence of inhibitor additives among the conditions reported to increase stray gassing (App. G.3, p. 62).
Four is not all of them (values and notes).
Copper moves hydrogen both ways
Two tables on one page of one brochure: two uninhibited service oils, same method, same 48 h, same 105 °C, same air, same copper. In one, copper takes hydrogen from 899 down to 527 µl/l. In the other, from 990 up to 1 381 µl/l (TB 927, Tables 8 and 9, p. 29).
Hydrogen goes both ways, so neither inhibition state nor service history tells you which way it will go. That is why the test runs with and without copper (ten more pairs).
Reference Figure 6 and ten more copper pairs
Figure 6 draws two pairs, service oils A and B; the tables below give those two and ten more, selected from the sources cited here, not every pair they print. All ran for 48 h. Service oil A is TB 927 case 2.4 (8 MVA, 35 kV, 13 years in service); service oil B is the 2020 network transformer of case 2.5 (§ 2.4, p. 28; Tables 8 and 9, p. 29).
Ethane rises with copper in every pair whose values the sources print where it reaches 1 µl/l. In the five IEC pairs that stay below 1 µl/l with and without copper it moves by 0.5 µl/l or less: up in two, flat in one and down in two (0.5 → 0.4 under nitrogen, Fig. A.3; 0.3 → 0.0 in air, Fig. A.4; IEC 60296:2020, pp. 30–32). In TB 927's soybean-ester chart, which prints no values, mean ethane in air is slightly lower with copper than without, and higher with copper under nitrogen; the error bars overlap (Fig. 8, p. 22; direction only, read from the chart). The rule above for ethane holds for the pairs whose values the sources print, all of them mineral oil.
| Liquid and condition | Without → with copper | Source |
|---|---|---|
| Uninhibited unused mineral oil, air, 105 °C | 0.8 → 163.5 µl/l ▲ | IEC 60296:2020, Fig. A.2, p. 29 |
| Service oil A (13 years in service), air, 105 °C | 100 → 194 µl/l ▲ | CIGRE TB 927:2024, Table 8, p. 29 |
| Service oil B (unit built 2020), air, 105 °C | 145 → 268 µl/l ▲ | CIGRE TB 927:2024, Table 9, p. 29 |
| Uninhibited service oil (unit 1-T7), nitrogen, 120 °C | 36 → 82 ppm ▲ | Buchacz et al. 2021, Fig. 11 table, p. 1733 |
Methane, same pairs: 223 → 267 and 162 → 303 µl/l (CIGRE TB 927:2024, Tables 8 and 9, p. 29); 50 → 68 ppm (Buchacz et al. 2021, Fig. 11 table, p. 1733). The eight IEC pairs are in the Figure 5 table.
TB 927 states both effects of copper. Its introduction lists among the main new findings that stray gassing is strongly catalysed by copper (§ 1.1, p. 9); four clauses later, among the assumptions behind the new test, it adds that copper can also quench the gas formation in some cases (§ 1.5, p. 13). In the pairs here the first holds for methane and ethane, the second for hydrogen in some oils; neither is a rule for hydrogen. That is why the test runs in pairs: copper's effect on hydrogen has to be measured on the oil in front of you. IEC 60296 adds that copper enhances the radical formation (Cl. 6.19, p. 20).
IEC 60296 uses copper because it is the winding metal in the majority of electrical equipment, and warns that the patterns may be somewhat different with enamelled windings or aluminium conductors (Cl. 6.19, p. 20). For a family wound mostly in enamelled copper, the field paper found the results without copper probably the more representative (Buchacz, p. 1734).
Hydrogen goes both ways.
| Liquid and condition | Without → with copper | Source |
|---|---|---|
| Uninhibited unused mineral oil, air, 105 °C | 5.3 → 82.8 µl/l ▲ | IEC 60296:2020, Fig. A.2, p. 29 |
| Inhibited mineral oil, triazolic passivator, air, 105 °C | 111.9 → 63.5 µl/l ▼ | IEC 60296:2020, Fig. A.3, p. 30 |
| Uninhibited recycled mineral oil, air, 105 °C | 262.4 → 290.0 µl/l ▲ | IEC 60296:2020, Fig. A.5, p. 32 |
| Uninhibited recycled mineral oil, nitrogen, 105 °C | 84.0 → 23.4 µl/l ▼ | IEC 60296:2020, Fig. A.5, p. 32 |
| Service oil A (13 years in service), air, 105 °C | 899 → 527 µl/l ▼ | CIGRE TB 927:2024, Table 8, p. 29 |
| Service oil B (unit built 2020), air, 105 °C | 990 → 1 381 µl/l ▲ | CIGRE TB 927:2024, Table 9, p. 29 |
| Uninhibited service oil (unit 1-T7), nitrogen, 120 °C | 77 → 30 ppm ▼ | Buchacz et al. 2021, Fig. 11 table, p. 1733 |
| Soybean-based natural ester, air | not printed; lower with copper (direction only) ▼ | CIGRE TB 927:2024, Fig. 8, p. 22 |
The soybean hydrogen panel is also printed in IEC 63585:2026 (Fig. 3 b), p. 13).
Natural and synthetic esters
The ester rows of the table, from Hanson et al. and IEEE C57.155, show that ethane is a property of the base oil, not of esters as a class (Hanson et al. 2016, Table III, p. 140; IEEE C57.155-2014, Table B.1, p. 16). In a natural ester, IEC 63585:2026 reads the trend of C₂H₄/C₂H₆: a significant rise in the ratio during operation "could suggest the possibility of an incipient high-temperature thermal fault" (Cl. 5.3.5, p. 19; above). The same clause says certain natural esters, those containing linolenic acid for example, can naturally develop relevant concentrations of ethane in the absence of a fault (Cl. 5.3.5, p. 19).
Linolenic content predicts ethane only loosely (why). A comparison needs the base oil and the additive package to be known first.
ℹ️ Note
Ester samples and light (Hanson et al. 2016). A week in direct sunlight took one natural ester sample to 1 380 ppm of hydrogen, 2 418 ppm of ethane and 114 ppm of ethylene, against 165, 2 and 0 on the laboratory counter. The authors write that "Proper storage of samples, in a closed cardboard box, for shipping and handling prior to processing is important". They add that the effect of light "under normal laboratory conditions appears to be small", while "samples stored in direct light during collection and transport could demonstrate dramatic shifts in results". For DGA samples in glass or rigid metal bottles, IEC 60475 asks for extra protection from light during transport and storage (Hanson et al. 2016, Table V, p. 141; § VII, p. 141; IEC 60475:2022, 4.2.5.1 a), p. 22).
Silicone
Silicone gives no stray gassing at 105 °C in the round robin, only hydrogen at 180 to 220 °C and very little at 250 °C (TB 927, p. 22; TB 771, App. G.6, p. 64; TB 443, Cl. 3.2, p. 9; note).
Reference What each temperature rests on
Temperature is the other half of the cross-fluid picture.
In temperature order, with what the source gives and how firmly:
| °C | Liquid | What the source gives | Source |
|---|---|---|---|
| 90 | Natural ester, soybean | already gassing, hydrogen-led (measured; oxygen supplied; no duration printed) | Hanson et al. 2016, Table IV, p. 140 |
| 105 | Mineral oil | the IEC 60296 acceptance condition (test condition) | IEC 60296:2020, A.4.3, p. 27 |
| 105 | Esters, both kinds | the soybean natural ester ethane-led; the synthetic ester's ethane sits at the axis (direction only) | CIGRE TB 927:2024, Figs. 7–8, pp. 21–22; IEC 63585:2026, Cl. 4.1.4, Figs. 3 and 5, pp. 13–14 |
| 105 | Silicone | no stray gassing (measured in the round robin) | CIGRE TB 927:2024, p. 22 |
| 120 | Mineral oil | mainly hydrogen, then methane, more or less markedly depending on the oil (measured) | CIGRE TB 296:2006, § 3.2, p. 12 |
| 120 | Natural ester, soybean | still gassing, with less hydrogen and more ethane than at 90 °C (measured; no duration printed; the values equal Table II's, which prints 1 day; ours) | Hanson et al. 2016, Table IV, p. 140 |
| 160 | GTL | reported to differ from naphthenic oils (reported, not verified: reference not held) | CIGRE TB 771:2019, App. G.3, p. 62 |
| 180–220 | Silicone | only hydrogen (stated; no data printed; App. D.1, p. 56, prints "> 200°C") | CIGRE TB 771:2019, App. G.6, p. 64 |
| 200 | Mineral oil | mainly methane and ethane, then hydrogen and ethylene (measured) | CIGRE TB 296:2006, Table 14, p. 12; § 3.2, p. 13; Annex C, Table C2, p. 28 |
| 250 | Silicone | very little (observed; no data printed) | CIGRE TB 443:2010, Cl. 3.2, p. 9 |
The soybean values behind the 90 and 120 °C rows: 1 060 ppm of hydrogen against 314 of ethane at 90 °C, and 448 of ethane against 403 of hydrogen at 120 °C; the samples were given oxygen before testing (Hanson et al. 2016, Table IV and § VI, p. 140).
See When the Fluid Changes the Diagnosis for which document applies to which fluid.
The test: can this transformer's oil make the gas?
The test that shows whether the oil itself can make the gas has to run on a sample from this transformer. Not the drum sample or the delivery certificate: the field paper's authors write that stray-gassing patterns of oils taken from drums and transformers are significantly different (Buchacz et al. 2021, p. 1729). The two results answer different questions: what the oil did as delivered, and what it does now. A difference between them is something to be explained, from this unit's history and from the tests themselves.
The test runs at 105 °C, which IEC 60296 calls the highest permissible top-oil temperature at normal cyclic loading. CIGRE degassed its 2020 network transformer's sample to "identify whether the gases are produced out of the oil (stray gassing)". TB 296 and the field paper degas too. IEC 60296, written for oil as delivered, does not filter or vacuum-treat its sample before purging (IEC 60296, Cl. 6.19, p. 20; TB 927, § 2.5, p. 29; IEC 60296, A.4.1 NOTE, p. 27).
Stray-gassing test on oil from this transformer, per CIGRE TB 927 § 1.6, as CIGRE did for in-service oil (§ 2.5).
- Degas the sample before saturation, without filtering, and state the method.
- Purge one portion 15 min with dry air (Procedure A). If the unit is sealed or nitrogen-blanketed, purge a second, separate portion 15 min with dry nitrogen (Procedure B).
- Incubate each portion 48 ± 0.5 h at 105 ± 2 °C, with and without copper.
- DGA per IEC 60567 (Annex F for ester).
- Report H₂, CH₄, C₂H₆, C₂H₄, C₂H₂, CO, CO₂, O₂ and N₂ in µl/l as sampled, after degassing and saturation, and after each incubation.
The test needs more oil than a routine DGA: each atmosphere fills two 50–60 ml syringes (TB 927, § 1.6.3.1, p. 14). Ask the laboratory how much it needs. The page behind each element of the test, what moves the pattern, and esters are in test provenance.
Reference Test provenance
- The test request, element by element. CIGRE's procedure purges for 15 minutes, fills two syringes of 50–60 ml per atmosphere, one with copper foils, runs 105 °C for 48 h and analyses per IEC 60567 (CIGRE TB 927:2024, § 1.6.3.1, p. 14). IEC 60296 sets the oven at 105 ± 2 °C (A.2, p. 26) and the duration at 48 ± 0.5 h (A.4.3, p. 27); its sample is not filtered or vacuum treated before purging (A.4.1 NOTE, p. 27). TB 927's procedure runs every oil in air and in nitrogen (§ 1.6.3, p. 14); the test request keeps nitrogen for sealed or nitrogen-blanketed units, the case TB 927 ties it to (§ 1.5, p. 13), and follows CIGRE's in-service precedent, air only, for a free-breathing unit (§ 2.5, Table 9, p. 29). A high oxygen content in nitrogen-saturated oil indicates leakage in the syringe, which is why O₂ and N₂ are reported (§ 1.7.1, p. 16). Esters are analysed per IEC 60567, Annex F (p. 60).
- The worked example. CIGRE ran this test on oil from the 2020 network transformer: degassed and air-saturated, the sample started near zero on hydrogen, the hydrocarbons and carbon monoxide, then gassed in both runs, more with copper (TB 927, § 2.5 and Table 9, p. 29). The unit is TB 927 case 2.5: "Network transformer, 25 MVA, 20 kV, manufacturing year 2020, uninhibited oil", sampled 2021. Table 9 holds its service values and its test values, the hydrogen of service oil B in Figure 6 (§ 2.5 and Table 9, p. 29).
- Why the sample is degassed. TB 296's procedure degasses under vacuum before saturating with air or nitrogen, and so did the field paper (TB 296, § 3.1.1, p. 11; Buchacz et al. 2021, p. 1730). The gas the unit put there has to be out before the test can show what the oil adds, which is why the values after degassing are reported (ours). Degassing is CIGRE's step for in-service oil, not an invention of ours.
- Degassing in service. In one CIGRE case ethane fell after degassing and rose again afterwards (TB 927, case 2.1, p. 25). In our reading, degassing the unit does not prevent the test, since the laboratory degasses the sample before saturation anyway (TB 927, § 2.5, p. 29).
- What moves the pattern. The field paper lists, among the factors that influence the pattern, the "time spent by the oil in the transformer in contact with transformer materials", beside test temperature, duration, air or nitrogen, copper, and syringes or vials (Buchacz et al. 2021, p. 1731).
- Esters. Esters take the same test request: where the liquid, construction materials or additives may influence the gas formation, IEC 63585 calls for a careful investigation and recommends the TB 927 test (Cl. 5.3.6, p. 19).
- Atmospheres. IEC 60296 air (procedure A) and nitrogen (procedure B); ASTM D7150 dry air and dry nitrogen; TB 296 air or nitrogen, after degassing; C57.155 an air sparge.
- Procedure origin. IEC 60296 credits the procedure to joint work of CIGRE WG D1.70 and IEC TC 10 (A.1, p. 26), and its Annex A is written for mineral oil (A.1, p. 26). CIGRE prints its own version as TB 927 § 1.6 (pp. 13–15) and notes that it has already been included in IEC 60296 (§ 1.2.2, p. 12). One difference matters when ordering: TB 927 purges the oil with air for 15 minutes (§ 1.6.3.1, p. 14), where IEC 60296 says only to purge it to saturation (A.4.1, p. 27).
- TB 296 detail. After 164 h the third syringe is degassed again, re-saturated with air or nitrogen and heated for another 16 h, to show whether the gassing recurs (§ 3.1.1, p. 11).
- Why one condition. The round robin found air with copper the most severe condition for gas formation, and the Table 3 limits are based on it (Cl. 6.19, p. 20). It is not the worst case for every gas: the passivated oil's hydrogen, air-saturated, is 111.9 µl/l without copper and 63.5 with it (Fig. A.3, p. 30).
Reference Stray-gassing tests compared: IEC 60296, ASTM D7150, CIGRE TB 296
Three methods go by the name "stray-gassing test", and a fourth reports ester data. Only one has a copper condition.
| Method | Conditions | Limit |
|---|---|---|
| IEC 60296 Annex A = CIGRE TB 927 § 1.6 | 105 °C · 48 h · with and without copper | > 50 µl/l H₂, CH₄ or C₂H₆ |
| ASTM D7150-13 | 120 °C · 164 h · no copper | none |
| CIGRE TB 296 | 120 °C (or 200 °C) · 16 h, 164 h, then a 16 h re-test · copper not specified | none |
| IEEE C57.155 Annex B* | 120 °C · 24 h · copper not printed | none |
*Inactive-Reserved; an informative ester comparison. IEC 60296 classes the oil "stray gassing" if the limit is exceeded in any condition. Sources: IEC 60296:2020, A.4–A.6, pp. 27–28; ASTM D7150-13, Cl. 1.1, 4.1, 7.7 and 9, pp. 1–2 and 5; CIGRE TB 296:2006, § 3.1.1–3.1.2, p. 11, and § 3.5, p. 15; IEEE C57.155-2014, Cl. 4.1.1, p. 5, and Table B.1, p. 16. TB 927's method is included in IEC 60296 (§ 1.2.2, p. 12); it purges 15 min, in air and in nitrogen (§ 1.6.3, pp. 14–15), and sets no limit of its own (§ 1.4, p. 13). In service, IEC 60599 points to two outside methods, TB 296 and ASTM D7150 (Cl. 4.3, p. 12, and its references [3] and [4]).
What counts as gassing is defined only for oil as delivered. For oil taken from a transformer, CIGRE writes that there are no criteria to compare this gassing to the eventual stray gassing of the oil (TB 927, § 1.4, p. 13), and its brochures do not agree on how far a laboratory result carries into service. We therefore read the test on service oil against the service DGA, not against 50 µl/l (the round robin and three CIGRE positions).
Reference What counts as gassing: the round robin and three CIGRE positions
IEC 60296 evaluates an unused or recycled oil as "stray gassing" if, under at least one tested condition, hydrogen, methane or ethane exceeds 50 µl/l (A.6.2, p. 28); oils treated on-site are outside its scope (Cl. 1, p. 8). The numbers are coarse: on oils as delivered, above 25 µl/l, the standard deviation was 30–80 % between the 18 laboratories of the round robin and 8–25 % within one (IEC 60296, A.7.2–A.7.3, p. 28). In classing those oils, 1 or 2 of 18 laboratories called a stray-gassing oil "non stray gassing", and none did the reverse (p. 29). How often the test misses on oil from a transformer has not been measured in any source cited here (ours).
TB 296 found that "In most cases, there is no correlation between test results at 120 °C and gassing observed in the field in the first year(s) of service", and in a few cases some correlation (§ 3.3, p. 13). TB 771 says "no stray gassing test can exactly simulate stray gas formation in transformers" and that such tests "should be used mainly to compare and classify different oils" (App. G.3, p. 62). TB 927, whose 105 °C method is the one ordered here, reports "similar gassing patterns of the same oil types" in the test and in transformer DGA (§ 1.1, p. 9). It uses the method in some service cases "for identification of the gas production as stray gassing" (§ 2, p. 24), and, for the oil of its case 2.4, concludes that "48 h of the test is long enough to adequatelly [sic] reproduce stray gassing of the oil" (case 2.4, p. 29). The same brochure says there is no criterion for comparing gas in service with the oil's stray gassing (§ 1.4, p. 13).
Not sure the pattern justifies the test, or how to specify it to your laboratory? Send us the DGA report, and we will come back with a proposal for a second opinion. The test can be arranged through a partner laboratory; it is not routine, so allow extra time.
When the answer is "it is stray gassing"
The answer may come as a comment on a DGA report, in a service or inspection report, or as a reply to a question about the unit. Whoever gives it, it is a conclusion to be shown on this transformer's oil, not a substitute for looking. In daily experience, CIGRE notes, "stray gassing is often invoked when the gassing pattern of a transformer is not clearly attributable to a fault, or when misleading DGA results are provided" (TB 927, § 1.3, p. 12). Ask to see what it rests on:
ℹ️ Note
What "it is stray gassing" has to rest on. Six conditions:
- Partial discharge investigated: a PD measurement on the unit if the point lies near the S/PD boundary (TB 771, App. G.2, p. 61).
- The other sources in the unit considered, whatever the test showed (IEC 60599, Cl. 4.4, p. 12).
- A test on oil from this unit, with and without copper and with its values after degassing, in which the oil makes the gases found in service in a comparable pattern, at 105 °C or at a stated test temperature matched to service (TB 927, § 2.5 and case 2.4, p. 29; Buchacz et al. 2021, p. 1732).
- Acetylene absent or, in a new or repaired unit, shown to come from a source that is not a fault, such as new stainless steel or welding, occurrences IEC 60599 calls very unusual (TB 927, § 1.7.1, p. 16; IEC 60599, Cl. 4.4, p. 12).
- Ethylene not rising, unless, in mineral oil, one of CIGRE's named causes fits; in a natural ester, C₂H₄/C₂H₆ not rising (TB 771, App. G.4, p. 62; IEC 63585, Cl. 5.3.5, p. 19).
- Where TB 296's rough check, a separate test at the unit's hottest-spot estimate, was run with the load history, the gas in service is not above its rough level (TB 296, § 3.5, p. 15; Table 16 notes, p. 14).
Only when all six hold can the oil, in our view, explain the gas. Even then it is not proven: below TB 296's rough level TB 296 cannot tell stray gassing from a T1 or T2 fault (§ 3.5, p. 15), and whether anything in the unit ran hotter than usual remains open. The oil's type and certificate, and a test on a retained sample of the delivered oil where one exists, show what the oil did before it entered the unit (Buchacz et al. 2021, p. 1729).
In one CIGRE case regeneration followed by inhibition removed the source of the gassing (TB 927, case 2.7, p. 30; the case); a test on oil that has since been regenerated and inhibited, or replaced, shows the oil as it is now.
What the standards recommend
The steps below are the standards' recommendations, not ours, and none of them is applied here to any unit. When gas concentrations and their rates of increase exceed typical values, IEC 60599 recommends increasing the sampling frequency (Cl. 9 c) 1), p. 21). Once a fault is identified in its procedure (Cl. 9 a), p. 21; Fig. 1, p. 23), IEC 60599 recommends considering complementary tests (acoustic, electrical, infrared) or reduced loading (Cl. 9 c) 2), p. 21). Depending on the results of complementary and other tests and on the advice of transformer experts, it recommends considering removing the transformer from service for inspection or repair (Cl. 9 c) 3), p. 21). Above alarm values of gas concentrations and rates of increase, it recommends considering immediate action (Cl. 9 c) 4), p. 21). IEC 63585 gives parallel steps for esters once abnormal gassing is detected (Cl. 10, p. 23). CIGRE TB 771 adds that these recommendations "are given for information only", and that actions on the equipment "are the sole responsibility of engineers in charge of the transformers" (App. C.8, p. 54; the ladder).
Reference What the standards recommend: the ladder and TB 771's levels
The rows below are the standards' recommendations, not ours, and none of them is applied here to any unit.
For stray gassing in power transformers, CIGRE TB 771 sets hydrogen levels of 460 ppm (typical), 800 and 1 100 ppm (intermediate 1 and 2) (Table 3.1, p. 17). For wind-farm transformers, whose hydrogen values IEC 60599 says "could not be inherently attributable to fault absence" (Table A.5, footnote c, p. 28), TB 771 says the Table 3.1 values "can therefore be significantly increased" (§ 3.2.1, p. 18).
| Source | Condition | Action |
|---|---|---|
| IEC 60599:2022, Cl. 1, p. 8 | All its indications | given "only as guidance with resulting action undertaken only with proper engineering judgment" |
| IEC 60599, Cl. 9 c) 1), p. 21 | Gas concentrations and their rates of increase exceed typical values | recommends increasing the sampling frequency (quarterly, monthly or other) |
| IEC 60599, Cl. 9 c) 2), p. 21 | No gas level of its own; in the procedure of Cl. 9 it follows the identification of a fault once at least one gas is above typical values of gas concentrations and rates of gas increase (Cl. 9 a); Fig. 1, p. 23) | recommends considering complementary tests (acoustic, electrical, infrared) or reduced loading |
| IEC 60599, Cl. 9 c) 3), p. 21 | Same procedure; "depending on the results of complementary and other tests and on the advice of transformer experts" | recommends considering removing the transformer from service for inspection or repair |
| IEC 60599, Cl. 9 c) 4), p. 21 | Gas concentrations and rates of gas increase exceed alarm values | recommends considering immediate action |
| IEC 60599, Cl. 9 a), p. 21 | Once a fault is identified | "Check for eventual erroneous diagnosis (see 4.3)", the clause on stray gassing |
| CIGRE TB 771, App. C.8, p. 54 | Stray gassing in power transformers, at TB 771's typical level (row 5 of the documented cases) | "increase oil sampling intervals from yearly to monthly, consider performing complementary tests (acoustic, electrical, infrared) or reduce loading" |
| CIGRE TB 771, App. C.8, p. 54 | At intermediate 1 | "increase oil sampling to weekly" |
| CIGRE TB 771, App. C.8, p. 54 | At intermediate 2 | recommends considering inspection, depending on the results of complementary tests |
| CIGRE TB 771, App. C.8, p. 54 | At pre-failure levels | "consider immediate action, removal from service for repair or replacement depending on damage observed" |
| CIGRE TB 771, Table 3.1 note, p. 17 | Stray gassing: no pre-failure value printed; calculated 2 840 ppm, with more than 15 cases between 8 400 and 55 000 ppm reported without failure | "a PF value much higher than this calculated PF value could probably be used in Table 3.1 and intermediate values 1 and 2 recalculated accordingly" |
| CIGRE TB 771, App. C.8, p. 54 | All the levels above | "these IEC recommendations based on gas levels (gas concentrations or gassing rates) are given for information only. Actual actions on the equipment are the sole responsibility of engineers in charge of the transformers" |
| IEEE C57.104-2019, Cl. 6.1.2.2, p. 36 | DGA Status 2 | possible causes "should be investigated"; where the fault diagnosis reveals PD, T1 or stray gassing, "this would be treated as a less urgent issue, but still may affect future life of the insulation system"; "Otherwise, increased sampling frequency should be maintained or started". Fig. 2 (p. 34) labels DGA Status 2 "Increased Transformer Surveillance and DGA Frequency" |
| IEEE C57.104-2019, Cl. 6.1.2.3, p. 37 | DGA Status 3: any one gas level above Table 2, or any rate above Table 4 (Step 6, p. 36) | "considered as probably suspicious"; probable causes "should be investigated"; "The transformer should be placed under increased surveillance and additional transformer testing is recommended. Consultation with the transformer manufacturer or a transformer expert is also recommended." If, after complete review, the condition is deemed acceptable for continuous operation, IEEE suggests surveillance typical of a lower DGA status |
| IEEE C57.104-2019, Cl. 6.1.2.4, p. 37 | Extreme DGA results: gas levels or changes "much larger than those provided in Table 2 and Table 3"; IEEE's examples are an increase in C₂H₄ of 200 µl/l or a level of C₂H₆ of 1 000 µl/l | "warrant immediate extra investigation"; "immediate investigation and operating restrictions should be initiated, at least until the cause of the large value is either dismissed as "erroneous" (sampling error for example) or fully understood and the unit has been deemed acceptable for continued operation" |
| IEC 63585:2026, Cl. 5.5, p. 20 | Esters, "Should a condition exist in the transformer which causes the gas formation"; "Trending is most often done when gas levels are relatively low"; and "in the majority of cases" | "the best course of action is to trend the production of these gases"; "trending is the appropriate action" |
| IEC 63585, Cl. 5.5, p. 20 | Esters, a high concentration of ethylene or acetylene in a single test | "can lead to the decision to take the unit out of service for further investigation" |
| IEC 63585, Cl. 10 a), p. 23 | Esters, "In case an abnormal gassing according to the applied interpretation schemes is detected", and gas-in-oil concentrations above the 90 or 95 percentile values (or other values based on justified utility or user experience) | recommends increasing the sampling frequency (weekly, monthly, quarterly or other), calculating rates of gas increase in µl/l/day and following their development and that of the gas-in-oil values |
| IEC 63585, Cl. 10 b), p. 23 | Esters, abnormal gassing detected | recommends considering complementary tests (acoustic, electrical, infrared) and/or reduced loading |
| IEC 63585, Cl. 10 c), p. 23 | Esters, abnormal gassing detected; depending on the results of complementary and other tests and on the advice of transformer experts | recommends considering removing the transformer from service for inspection or repair |
What we recommend
IEEE C57.104 on a second sample. For DGA Status 2, IEEE C57.104 says: "Resample for confirmation and monitor possible gas evolution" (Cl. 5.3, p. 28). For a new or repaired unit it adds that a diagnosis "cannot be considered unless a second sample confirms active fault gas production in a pattern that confirms the diagnosis" (Cl. 5.3.1, p. 29).
Read the report:
- Gate on acetylene. Stray gassing does not explain acetylene (when to test).
- The liquid, its base oil and its additives set which gas leads in the test (your liquid).
- Read ethylene by trend, not by presence (against a thermal fault).
- Use the ratio and the Duval zones as an indication, never as the decision. Where the diagrams disagree on one sample, CIGRE's reading is that this may be an indication of multiple faults (TB 771, App. H.4, p. 69; IEEE C57.104, Annex D.7, p. 69): stray gassing and a fault can be present together (when the diagrams disagree). IEEE C57.104 writes: "It is not recommended to attempt fault identification using the methods described in 6.2 and Annex D if all of the gas levels are below the Table 1 values" (Cl. 5.2.1, p. 27). For esters, IEC 63585 warns of "misleading results" when all gases are significantly below its 90th or 95th percentiles (Cl. 5.1, p. 16).
- Look for the plateau and for falling oxygen. One sample shows neither (what each sign settles).
Reference When the diagrams disagree
When it discusses mixtures of faults, IEEE C57.104 explains why the diagrams disagree on one sample: each graphical representation is more sensitive to some gases and some faults than to others; for example, Triangle 4 and the Pentagons are more sensitive to H₂ and to faults S and PD, while Triangles 1 and 5 are more sensitive to C₂H₄ and faults T3 (IEEE C57.104-2019, Annex D.6, p. 68). It says this of the mineral-oil diagrams only.
CIGRE shows two inspected cases in which a mixture of faults put the point in zone S. When an overheating fault moved to a D1 discharge in oil, with 317 ppm of acetylene, "the DGA point appears temporarily and inappropriately in zone D2 of Triangle 1 and in zone S of Pentagon 2, because of the mixture of faults and gases" (TB 771, Table 3.13 and note, p. 23). A 230 kV bushing with 9 to 21 ppm of acetylene, placed in S by Triangle 4 and in S/D1 by Pentagon 2, had "multiple faults: partial discharges of the sparking type D1 in paper (carbonized punctures), T3-H fault on metal part in oil, and stray gassing S of surrounding oil" (Table 3.27 and note, p. 30). Both carried acetylene, which the first step of the reading already gates on (ours).
For what comes after, CIGRE and IEEE describe the same method: where the point moves in the diagrams, the previous results are subtracted from the latest, negative differences are set to zero, and the difference is read as the new source (TB 771, App. H.6, p. 70; IEEE C57.104, Annex D.6, p. 68). IEC 60599 likewise has the previous DGA values subtracted from the last ones before the ratios are recalculated (Cl. 6.1 d), p. 17).
The other sources and the test:
- Other sources in the unit, whatever the test shows. IEC 60599 lists steel or galvanised steel with water, some stainless steels, coatings, paints, welding and sunlight, and calls these occurrences very unusual (Cl. 4.4, p. 12; the list).
- Where stray gassing is to be shown, order the stray-gassing test on oil from this transformer (the test request).
Reference Other sources in the unit
IEC 60599 lists other sources of gas: steel and galvanised steel reacting with water, as long as oxygen is available ("Large quantities of hydrogen have thus been reported in some transformers that had never been energized"); free water with special coatings on metal surfaces; some types of stainless steel; gases absorbed in new stainless steel or produced by welding and released slowly into the oil; internal paints; and exposure of the oil to sunlight. It calls these occurrences "very unusual" and says they "can be detected by performing DGA analyses on new equipment which has never been energized, and by material compatibility tests" (Cl. 4.4, p. 12). IEEE C57.104 adds catalytic reactions (R) "between water and galvanized steel in oil sampling valves of transformers or with tank stell [sic] (rust)", which it calls very rare (Annex C.2, p. 60). IEC 60296 and CIGRE keep gas from incompatible materials outside the definition of stray gassing (IEC 60296, Cl. 6.19, p. 20; TB 927, § 1.5, p. 13).
IEC 60599 is written for mineral oil and applies to other liquids only with caution (Cl. 1, p. 8); the list is read with that caution for an ester.
In the washer family both oils gassed in the laboratory, and the authors still traced the high hydrogen to galvanised steel washers in the units (Buchacz et al. 2021, pp. 1732–1734).
Act on the answer:
- If the oil does not gas in the test, the test does not support stray gassing. It does not rule it out. Re-open partial discharge and T1/T2.
- If the oil gasses in the test, whether it made this unit's gas is still to be shown. The test characterises the oil, not the transformer: the oil can be a source of the gas, and what else remains open is in the checklist.
- Report the assessment in two parts: what is still open on the unit, and, only if the gas is shown to be stray gassing, how IEC 60599 classes it. Whether anything in the unit ran hotter than usual is still to be shown. If the gas is shown to be stray gassing, IEC 60599 classes it as a non-damage fault, one with no repair or replacement at the point where it forms (IEC 60599, Cl. 4.3, p. 12; Cl. 3.1.2, p. 9).
See Step 4 of Navigating the DGA Maze for where this sits in the wider workflow.
Holding a DGA report that reads like stray gassing? Send us the report and we will come back with a proposal for a second opinion. We interpret and advise. The test can be arranged through a partner laboratory; it is not routine, so allow extra time.
Buying oil: what "non stray gassing" on a certificate covers
For a Type A oil (fully inhibited, the grade with the higher oxidation stability; Cl. 5.1.1, p. 13), IEC 60296 sets the limit on one condition, air-saturated oil with copper: below 50 µl/l each of hydrogen, methane and ethane (Table 3, p. 21). Annex A evaluates an oil as "stray gassing" if any of the three gases exceeds 50 µl/l under at least one of the conditions that were run (A.6.2, p. 28). A "non stray gassing" certificate therefore speaks only for the conditions it rests on (why the two can differ). Under IEC 60296, a Type B oil, the grade that includes every uninhibited oil (Cl. 5.1.1, p. 13), carries the stray-gassing test, and any limit, only where user and supplier have negotiated them (Table 4 footnote, p. 24). IEC 60296's test does not consider gassing from incompatible materials; in the standard's words, "The method used in this document and described in Annex A does not consider this, since the compatibility of materials is a responsibility of the equipment manufacturer" (Cl. 6.19, p. 20).
Reference What a certificate does not cover
The Table 3 condition, air-saturated oil with copper, is the one the round robin found "the most severe condition for gas formation", and "The limits reported in Table 3 are based on the testing under this condition" (IEC 60296, Cl. 6.19, p. 20). Annex A recommends all four conditions for a new type of oil, while for a new batch "testing with procedure A with copper can be sufficient" (A.6.2, p. 28). The two agree when only air with copper is run. They need not agree when more is run: the round robin's passivated oil gave more hydrogen without copper (111.9 µl/l) than with it (63.5) (Fig. A.3, p. 30). In our reading, an oil can therefore stay below 50 with copper and exceed it without. Type B, which includes every uninhibited oil, has no limit: "there has been insufficient data to determine appropriate limits" (Table 4 footnote, p. 24). IEC 60296 adds that the characterization "should be considered when users select an oil for equipment so that it forms part of the supporting information when DGA is done", and that testing in air and nitrogen, with and without copper, "can be beneficial for qualifying a new oil" (Cl. 6.19, p. 20). Among mineral oils, uninhibited ones show the stronger tendency to stray gassing (TB 927, § 1.1, p. 9).
At exactly 50 µl/l the two wordings differ: Table 3 asks for less than 50, A.6.2 for not more than 50 (ours).
Reference Glossary
- Stray gassing (IEC 60296). Gas formed in an insulating liquid in service "under temperatures considered usual for normal operating conditions … due to its constituents and not connected to an internal fault in the electrical equipment" (IEC 60296:2020, Cl. 6.19, p. 20).
- Stray gassing (CIGRE 2006). "the formation of gases from insulating mineral oils heated at relatively low temperatures (90-200 °C)" (TB 296:2006, § 3, p. 11).
- S, zone S. The stray-gassing zone of Triangle 4 and Pentagons 1 to 3; IEEE's abbreviation: "Stray gassing at temperatures < 200 °C" (IEEE C57.104-2019, Table C.2, p. 60).
- PD, partial discharge. "electric discharge that only partially bridges the insulation between conductors"; the DGA fault class PD is partial discharges "of the cold plasma (corona) type, resulting in possible X-wax deposition on paper insulation" (IEC 60599:2022, Cl. 3.1.7, p. 9; Cl. 5.3, p. 13).
- Corona PD, corona-type PD. The same class as PD above. IEC 60599: corona is "a form of partial discharge that occurs in gaseous media around conductors that are remote from solid or liquid insulation". Sparking-type partial discharges are classed with D1, not PD (IEC 60599, Cl. 3.1.7 Note 3, p. 9; Cl. 5.3, p. 13).
- T1. "Thermal fault t < 300 °C" (IEC 60599, Table 1, p. 14).
- T2. "Thermal fault 300 °C < t < 700 °C" (IEC 60599, Table 1, p. 14).
- Zone O. "Overheating < 250 °C without carbonization of paper" (IEEE C57.104, Table C.2, p. 60).
- Zone C. "Possible paper carbonization"; "a possibility of carbonization of paper, not a 100% certainty" (IEEE C57.104, Table C.2, p. 60; Annex D.5 NOTE, p. 67).
- Triangle 4. Duval's triangle for low-temperature faults in mineral oil, plotted from H₂, CH₄ and C₂H₆, used only after Triangle 1 has placed the sample in PD, T1 or T2 (IEEE C57.104, Fig. D.3 and Table D.3, p. 65; Annex D.4 note b), p. 66).
- Pentagon 1. Duval's first pentagon for mineral oil, showing the six basic fault types and stray gassing S (TB 771:2019, App. H.3, p. 69).
- Pentagon 2. Keeps Pentagon 1's electrical zones and splits the thermal ones into S, O, C and T3-H; plotted from H₂, CH₄, C₂H₆, C₂H₄ and C₂H₂ (IEEE C57.104, Annex D.5 and Fig. D.5, p. 67).
- Pentagon 3. Duval pentagons for esters, whose S zone changes shape from one ester to the next (TB 771, App. G.6, p. 64).
- Uninhibited oil (U). "mineral insulating oil containing no oxidation inhibitor or other antioxidant additives" (IEC 60296, 3.5, p. 11).
- Inhibited oil (I). "mineral insulating oil containing a minimum of 0,08 % and a maximum of 0,40 % of total inhibitor content as measured in IEC 60666" (IEC 60296, 3.7, p. 11).
- Passivator, passivated oil. Passivator: "additive used primarily as corrosion deactivator and sometimes as electrostatic charging depressant"; a passivated oil is one containing it (ours) (IEC 60296, 3.4.2, p. 11).
- Type A. "fully inhibited ("I" according to 5.1.2) and deliver higher oxidation stability than Type B" (IEC 60296, 5.1.1, p. 13).
- Type B. "can be uninhibited ("U"), trace inhibited ("T") or fully inhibited ("I")" (IEC 60296, 5.1.1, p. 13).
- Degas. Remove the gas dissolved in the oil, under vacuum in TB 296's procedure (TB 296, § 3.1.1, p. 11).
- Purge, sparge. Bubble air or nitrogen through the oil: "purge it with air to ensure saturation" (IEC); "purge it for 15 min with air" (CIGRE); ASTM D7150's sparge is 30 min with dry air (IEC 60296, A.4.1, p. 27; TB 927, § 1.6.3.1, p. 14; ASTM D7150-13, Cl. 4.1, p. 1).
- Saturate. The end of the purge: the oil holds as much of that gas as it will dissolve (ours, plain meaning; no source defines it).
- µl/l and ppm. The same unit for dissolved gas, microlitres of gas per litre of oil: "All values are in µl/l (ppm)" (TB 927, Table 9 caption, p. 29).
- Non-damage fault. "fault which does not involve repair or replacement action at the point of the fault"; IEC's examples include "stray gassing of oil" (IEC 60599, Cl. 3.1.2 and Note 1, p. 9).
- Fault (IEC 60599). "unplanned occurrence or defect in an item which may result in one or more failures of the item itself or of other associated equipment" (IEC 60599, Cl. 3.1.1, p. 8).
Sources
Page numbers are those printed in each document.
- Buchacz T., Buchacz J., Duval M. "Stray Gassing of Oil in HV Transformers." IEEE Transactions on Dielectrics and Electrical Insulation, vol. 28, no. 5, October 2021, pp. 1729 ff. DOI 10.1109/TDEI.2021.009520.
- Hanson D., Li K., Plascencia J., Beauchemin C., Claiborne C., Cherry D., Frimpong G., Luksich J., Lemm A., Martin R. "Understanding Dissolved Gas Analysis of Ester Liquids: an Updated Review of Gas Generated in Ester Liquid by Stray Gassing, Thermal Decomposition and Electrical Discharge." 2016 Electrical Insulation Conference (EIC), Montréal, Qc, Canada, 19–22 June 2016, pp. 138 ff.
Frequently asked questions
What is stray gassing in a transformer, and is it a fault?
What does ethane mean in a natural-ester transformer?
How do I tell stray gassing from partial discharge?
How do you test transformer oil for stray gassing?
What does 'non stray gassing' mean on an oil certificate?
Hydrogen came back after degassing. Does that mean a fault?
Why is there hydrogen in a new transformer?
Standards referenced
The methods on this page are anchored in these standards — follow each into our standards library.
Put Theory into Practice